| HS Code | 671131 |
| Polymer Type | High Density Polyethylene |
| Density | 0.950 g/cm³ |
| Melt Flow Rate | 7.5 g/10 min (190°C/2.16 kg) |
| Tensile Strength At Yield | 28 MPa |
| Elongation At Break | 600% |
| Flexural Modulus | 1100 MPa |
| Notched Izod Impact Strength | 60 J/m |
| Vicat Softening Temperature | 125°C |
| Heat Deflection Temperature | 70°C |
| Shore D Hardness | 65 |
| Melting Temperature | 130°C |
| Crystallization Temperature | 115°C |
| Water Absorption | <0.01% |
| Environmental Stress Cracking Resistance | >1000 h |
| Bulk Density | 0.55 g/cm³ |
As an accredited ZPC (Zhejiang Petroleum & Chemical) HDPE 7750M2 / GF7750M2 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | ZPC HDPE 7750M2/GF7750M2 is supplied in 25 kg PP woven bags or 1000 kg jumbo bags, with 25 MT per 20-ft container. |
| Container Loading (20′ FCL) | 20′ FCL loading: ZPC HDPE 7750M2/GF7750M2, 25kg bags, palletized, shrink-wrapped, secured; approx. 25 MT net. |
| Shipping | ZPC HDPE 7750M2 / GF7750M2 is shipped as non-hazardous, solid polyethylene resin pellets. Standard packaging: 25 kg PP bags or 1 MT jumbo bags, palletized and containerized. Not classified as dangerous goods. Store dry, ventilated, away from heat, direct sunlight, and contamination during sea, road, or rail transport. |
| Storage | Store ZPC HDPE 7750M2/GF7750M2 in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, ignition sources, and moisture. Keep original bags sealed and palletized to prevent contamination, dust, and UV degradation. Avoid strong oxidizers, protect from physical damage, maintain stable ambient temperature, and use first-in, first-out stock rotation with clean handling and no smoking. |
| Shelf Life | ZPC HDPE 7750M2/GF7750M2 typically has a 12-month shelf life when stored unopened, cool, dry, ventilated, and away from direct sunlight. |
For potable water networks, ZPC HDPE 7750M2 is extruded into solid-wall pressure pipe on a single-screw line with a grooved feed bushing and a spiral-mandrel or basket die. The GF7750M2 variant is supplied as a black compound for outdoor storage; the non-GF grade is processed where natural material or in-house colouring is specified. ISO 4427-1 requires black pipe intended for outdoor exposure to contain carbon black at 2.0–2.5% by mass, with particle dispersion no worse than grade 3 when assessed according to ISO 18553. Oxidative stabilisation is verified by oxidative induction time testing under ISO 11357-6; for PE100 pipe compound the OIT at 200 °C is expected to be not less than 20 min. A conservative quality plan checks OIT both on virgin pellet and after extrusion because thermal history can consume antioxidant reserves.
Moisture uptake in HDPE is low, but cold-warehouse pellets can carry superficial condensation. A dehumidified-air hopper set at 70 °C to 80 °C for 1 h to 2 h is sufficient to remove surface moisture; desiccant drying is not normally required. The extruder should provide an L/D ratio of 30:1 to 36:1 and a compression ratio of 3.0:1 to 3.5:1. Barrel zones are commonly set from 160 °C to 180 °C in the feed section, 180 °C to 200 °C in the compression and metering sections, and 195 °C to 210 °C at the adapter head and die. The melt temperature measured at the adapter should not exceed 220 °C during continuous production. Melt pressure before the screen changer typically falls between 15 MPa and 35 MPa depending on the die restriction and output rate; pressure fluctuations above ±2% often indicate unstable feeding or worn screw elements.
Forming and calibration are carried out with a vacuum sizer and spray or immersion cooling. The cooling water temperature is held between 15 °C and 30 °C; too low a temperature increases frozen-in stress, while too high a temperature reduces line speed stability. The haul-off speed is controlled by the wall-thickness scanner and must produce a minimum wall thickness that satisfies the selected standard dimension ratio. For PE100 water pipe, the nominal pressure rating follows the relationship between the minimum required strength of 10.0 MPa and the SDR. A pipe with SDR 11 is typically rated at 16 bar for water at 20 °C, SDR 17 at 10 bar, and SDR 26 at 6.3 bar, subject to the design coefficient applied in the local standard. The hydrostatic design basis is established by long-term pressure testing under ISO 9080:2012 and the material is classified as PE100 under ISO 12162:2009 when the lower confidence limit at 50 years and 20 °C remains not less than 10.0 MPa.
The slow crack growth resistance of the finished pipe is verified with the notched pipe test of ISO 13479:2009. This is not a routine production test but it forms part of type approval and is relevant for pipes installed by open-cut and directional drilling. The installation contractor should not exceed the allowable pulling force determined from the pipe cross-section and the manufacturer’s safe pull stress; in practice a maximum tensile stress of 10 MPa during pull-in is often used as a conservative ceiling for PE100, but the exact limit must be calculated for each SDR. For North American potable water contact, NSF/ANSI/CAN 61 certification is required; for Australia, AS/NZS 4020 is commonly referenced. Organoleptic compliance is separate from mechanical compliance and must be confirmed for the exact pigments used in non-black 7750M2 pipe.
The gas distribution use case is governed by ISO 4437 and, in North America, ASTM D2513. These standards do not rely solely on melt flow rate or density; they require proof of long-term hydrostatic strength, slow crack growth resistance, and rapid crack propagation resistance. For ZPC GF7750M2, the black compound provides the UV stabilisation needed during open-yard storage. Gas pipes are normally identified by yellow markings on a black pipe or by a co-extruded yellow layer; the identification requirements are part of the standard and must not be treated as decorative. The MRS classification remains 10.0 MPa, but gas network operators often specify SDR 11 or SDR 17 for distribution mains depending on the maximum operating pressure. At 20 °C, SDR 17 PE100 pipe is commonly rated up to 8 bar and SDR 11 up to 10 bar or higher under specific operator conditions.
Rapid crack propagation is a critical concern for gas piping because a crack can propagate at high speed along a pressurised line. Full-scale and small-scale tests are specified; the S4 test of ISO 13477 is commonly used for material qualification. The pipe supplier should provide the critical pressure and critical temperature data for the specific diameter and wall thickness. Slow crack growth is separately confirmed by the notched pipe test according to ISO 13479. In addition, the melt flow rate of the resin is checked under ISO 1133-1:2022 at 190 °C with 5 kg load, because a shift in MFR indicates thermal degradation or the presence of rework outside the approved ratio. Carbon black dispersion is checked to ISO 18553, and oxidative induction time is checked to ISO 11357-6. The gas distribution network operator normally requires these results on a lot-by-lot basis, not only at type approval.
Butt fusion joining follows ISO 21307 or the operator’s approved procedure. The fusion pressure and time are derived from the pipe diameter and SDR, not from generic heating-plate settings. The heater plate surface temperature is usually between 200 °C and 230 °C; thermocouple verification of the plate surface is mandatory because a drop of 10 °C changes the melt bead formation. The pipe must be scraped, aligned, and faced immediately before heating. Typical interfacial fusion pressure for PE is 0.15 MPa, with machine gauge pressure adjusted for cylinder area; precise values must be taken from the machine manufacturer’s tables or the pipe maker’s weld procedure. The presence of heavy condensates or odorants in gas service does not remove the requirements for pressure de-rating at higher temperatures. Hydrogen blending is currently under evaluation in many networks; published data for this specific grade under sustained hydrogen exposure is limited, so design qualification for hydrogen service should not proceed without additional material-specific testing.
| Application zone | Governing standard | Key test method | Parameter controlled |
|---|---|---|---|
| Potable water pressure pipe | EN 12201-2, ISO 4427-2 | ISO 1167-1 | Hoop stress, 20 °C and 80 °C |
| Gas distribution pipe | ISO 4437, ASTM D2513 | ISO 13477, ISO 13479 | RCP and slow crack growth |
| Spiral-wound profile pipe | ASTM F894, EN 13476-3 | ISO 9969 | Ring stiffness |
| Mining slurry line | ASTM F714 | ISO 13479 | Notched pipe slow crack growth |
| Sewer force main | EN 12201-2 | ISO/TR 10358 | Chemical derating factor |
Profile-wall pipe produced by spiral winding imposes a narrower process window than conventional solid-wall pipe because the product depends on fusion at the overlap of a continuously extruded profile strip. Large-diameter HDPE pipe from 300 mm to 3,000 mm is built by winding a heated profile onto a rotating steel drum, with adjacent helical edges fused under controlled pressure. The ZPC grade is suitable for this process only if the melt temperature at the contact point remains above the crystalline freeze point long enough to allow interdiffusion. In practice, the surface temperature at the overlap should not fall below 130 °C before the pressure roller compresses the seam; above 220 °C, oxidation accelerates and the antioxidant package is consumed too rapidly for storage tanks and buried pipe service. The operating window is therefore narrow and is often controlled within ±5 °C when ambient conditions are variable.
The extruder used for the profile strip is typically a grooved-feed single-screw machine with L/D 30:1 to 36:1, and a melt pump is recommended to damp pressure surges from the winder. Die exit melt temperature is kept from 195 °C to 215 °C. The drum and strip temperature are preheated to 80 °C to 120 °C; larger drums require the upper end of this range to prevent freeze-off between the die and the winding point. Roller pressure must be set so that the seam is fully consolidated without reducing the profile height. Excessive roller force flattens the wall and lowers ring stiffness; insufficient roller force produces a visible seam with poor fusion that may delaminate under buried load. Ring stiffness is verified according to ISO 9969 or the equivalent national method. A typical buried stormwater or drainage installation specifies SN4 or SN8, but the SN value alone is insufficient; the pipe must also meet long-term creep modulus assumptions used in the structural design.
Output rates in spiral winding are limited not by the extruder alone but by the heat removal from the seam. Because the profile is repeatedly reheated and cooled, the stabiliser system is subjected to multiple thermal cycles. Quality control should include OIT on the finished pipe wall at the seam and at the profile core. The external black GF7750M2 variant can be used for above-ground sections, while the natural 7750M2 may be co-extruded to permit welding inspection. Cut lengths and field welding are performed by butt fusion on the solid wall ends or by extrusion welding on the helical seam; extrusion-weld procedures for large-diameter HDPE structures must be qualified by a procedure test and inspected by bend tests and visual bead criteria.
Hard-rock mine tailings pipelines specify HDPE 7750M2 for above-ground temporary lines and permanent gravity return lines where the wet-sliding abrasion environment degrades steel quickly. The design basis for pressure load remains the PE100 hydrostatic design basis, but the line pressure may be de-rated for elevated temperature and chemical species using ISO/TR 10358. A flow velocity above 4 m/s during continuous tailings transport can produce sliding-bed wear concentrated in the invert; pipe rotation every 6 to 12 months is used in many operations to distribute wear before replacement. The specific abrasion rate for this grade in high-solids slurry is not published in a code-enforceable form, so the wall-thickness allowance must be derived from site-specific mass-loss data or a pilot loop. HDPE does not corrode by sulfide attack, but the outer wall above-ground requires the carbon-black-stabilised GF7750M2 variant for UV resistance. When flanges and mechanical couplings are used in temporary mine lines, the clamping pressure must not reduce the pipe cross-section below the minimum wall thickness required for the design pressure, and the coupling manufacturer’s pull-out resistance should be validated on the actual pipe OD.
When extruded into corrugated or smooth-wall HDPE conduit for underground power and communication cable protection, ZPC 7750M2 can be processed on a standard grooved-feed single-screw line with vacuum calibration; UL 651A is the applicable North American product standard for HDPE conduit, and the finished duct must meet the impact and crush resistance tests of that standard.
In sanitary force-main installations, the pipe operates as a pressure line carrying screened or unscreened sewage, often with residual hydrogen sulfide and chloride species. The PE100 classification still supplies the long-term strength basis, but the operating pressure is multiplied by a chemical resistance derating factor selected from ISO/TR 10358. Selection requires the continuous chemical class, concentration, and pipe wall temperature; a room-temperature municipal sewage service with dilute sulfide may allow a factor near 1.0, whereas acidic or solvent-laden industrial effluent may reduce the allowable stress to 0.8 or lower. The pressure derating for temperature follows the PE100 design coefficients; at 30 °C the reference factor is approximately 0.87, and at 40 °C it falls to approximately 0.74. These factors are design rules, not material properties, and they must be applied before selecting the SDR.
Unlike reinforced concrete or cast iron, HDPE force-main pipe is not consumed by biogenic sulfuric acid attack in the crown space, but the wall must still be checked for external soil load and vacuum transients. Ring flexibility tests according to ISO 9969 or equivalent are part of the product specification. When the line is installed by directional drilling, the allowable pulling force and bending radius must be based on the pipe manufacturer’s published values for PE100 and the specific SDR. The use of the black GF7750M2 variant is appropriate for above-ground valve chambers and creek crossings, but buried force mains may use either black or natural 7750M2 depending on the owner’s specification. Because sulfide, soap, and grease are present in the sewage matrix, the lot-specific slow crack growth resistance from ISO 13479 should remain on file; it is a better indicator of long-term performance in this service than short-term tensile properties.
Competitive ZPC (Zhejiang Petroleum & Chemical) HDPE 7750M2 / GF7750M2 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
ZPC (Zhejiang Petroleum & Chemical) HDPE 7750M2, also designated GF7750M2 in gas-phase reactor documentation, is a bimodal high-density polyethylene resin produced at the Zhoushan integrated refining and petrochemical complex. The product is intended for pressure pipe extrusion and appears in water distribution, industrial fluid transport, and gas distribution applications where the pipe compound is qualified under ISO 12162 as PE100 class. The two designations refer to the same base resin: GF7750M2 appears in production and export documentation for the gas-phase train, while HDPE 7750M2 is commonly used in domestic extrusion specifications. Melt flow rate measured according to ISO 1133-1 at 190 °C under a 5.0 kg load is typically reported within 0.20–0.30 g/10 min, a range that prevents melt sag during large-diameter pipe extrusion but still permits sufficient output in a grooved-feed extruder. Density determined by ISO 1183-1 is normally cited from 0.950 g/cm³ to 0.958 g/cm³, supplying a balance of stiffness and slow crack growth resistance. Tensile yield stress by ISO 527-2 is reported as not less than 22 MPa, with elongation at break above 600%.
These values differentiate the grade from injection-moulding HDPE resins with higher melt flow and from lower-density polyethylene pipe materials. The resin is supplied as natural or carbon-black-compounded pellets. In pressure pipe, the carbon-black variant provides ultraviolet screening, while the natural variant is suitable for industrial lines where no UV exposure is specified. The pellet form remains suitable for single-screw extrusion, spiral mandrel dies, and co-extruded multilayer pipe structures utilising the same PE100 class as the inner or middle layer.
Processing behaviour for 7750M2 is constrained by the same rheological trade-off that governs all bimodal PE100 resins. In a grooved-feed single-screw extruder with a 30:1 L/D barrier screw and a Maddock mixing section, the resin is commonly processed with a barrel temperature profile of 180–210 °C and a head/die temperature of 195–215 °C. Melt pressure before the screen pack is typically maintained between 250 bar and 400 bar (25–40 MPa) to ensure homogenisation without excessive shear heating. The high shear sensitivity of the high-molecular-weight fraction means that screw speeds above 80 rpm on 75 mm or 90 mm extruders can drive local melt temperature beyond 230 °C, leading to antioxidant consumption, gel defects, and inner-wall oxidation marks. A positive-displacement melt pump between screw tip and die is recommended for large-diameter pipe to reduce surging; pump inlet pressure is typically controlled at 50–80 bar, and pump outlet pressure is set to maintain constant die throughput. Die swell is approximately 1.2–1.4 at a shear rate of 100 s⁻¹ and should be accounted for when sizing the mandrel and outer die diameter.
The melt should be screened through a 40/60/80 mesh pack to remove unmelt particles and carbon agglomerates. An oscillatory frequency sweep from 0.01 rad/s to 100 rad/s at 190 °C should be used to determine the crossover modulus and the terminal relaxation time; a shift in these parameters relative to a reference lot can indicate a change in the high-molecular-weight fraction or contamination. Published data for GF7750M2 in spiral mandrel die configurations with barrier screws above 90 mm diameter is limited; processors should therefore perform a resin qualification run with a small-scale rheometer and pipe hydrostatic test before changing die geometry.
On a molecular level, the bimodal distribution in 7750M2 provides a distinct distinction from unimodal HDPE in slow crack growth. In pipe service, slow crack growth occurs when a crack tip propagates through the amorphous phase; tie molecules that bridge adjacent lamellae must be stressed to failure. The high-molecular-weight fraction of 7750M2 raises the probability that tie molecules remain entangled between crystalline lamellae. This is reflected in notched pipe testing according to ISO 13479: PE100-class formulations generally exceed 500 h at 80 °C under the class hoop stress, whereas PE80 unimodal materials often fail between 100 h and 500 h. Because GF7750M2 is bimodal, the high-molecular-weight fraction also contains a controlled amount of short-chain branching; this reduces crystallinity slightly and increases ductility. Published direct comparative comonomer placement data for this specific product is limited, but the performance envelope is consistent with hexene-copolymerised PE100 pipe resins.
Long-term hydrostatic strength classification of 7750M2 follows ISO 9080 regression using multiple rupture points across 20 °C, 60 °C, and 80 °C. For ISO 12162 PE100 classification, the lower predictive limit at 50 years and 20 °C must remain above 10 MPa. Qualification pipes are often 32 mm SDR11 specimens; acceptance points include 100 h at 20 °C under 12.4 MPa hoop stress and 1,000 h at 80 °C under 5.4 MPa hoop stress. The resin’s oxidative induction time measured by ISO 11357-6 at 210 °C is maintained above 20 min for natural pellets and above 15 min for carbon-black-compounded variants. This OIT threshold is not a direct field-life indicator but is used to monitor process heat history and residual antioxidant concentration. A drop in OIT below 15 min after extrusion indicates excessive melt temperature, insufficient antioxidant dispersion, or contaminated regrind.
| Property | Test method | ZPC 7750M2 / GF7750M2 | PE80 unimodal reference | General-purpose injection HDPE |
|---|---|---|---|---|
| Melt flow rate at 190 °C, 5.0 kg | ISO 1133-1 | 0.20–0.30 g/10 min | 0.40–0.70 g/10 min | 5–20 g/10 min |
| Density | ISO 1183-1 | 0.950–0.958 g/cm³ | 0.945–0.952 g/cm³ | 0.955–0.965 g/cm³ |
| Tensile yield stress | ISO 527-2 | ≥22 MPa | ≥20 MPa | ≥25 MPa |
| Elongation at break | ISO 527-2 | ≥600% | ≥600% | 100–400% |
| Notched slow crack growth at 80 °C | ISO 13479 | >500 h under class hoop stress | 100–500 h | Not applicable |
| MRS classification | ISO 12162 | 10 MPa | 8 MPa | Not applicable |
| Oxidative induction time at 210 °C | ISO 11357-6 | >20 min natural | >20 min | Not typically specified |
Thermal and chemical boundaries for GF7750M2 require strict handling in warehouse and processing areas. Pre-drying at 80 °C for 2 h is required if the pellets have been stored above 60% relative humidity or have undergone condensation from temperature cycling. Regrind levels above 10 wt% should not be used in pressure pipe intended for 50-year service unless the lot is re-qualified by hydrostatic testing. The resin should not be combined with amine-based stabilisers or excessive peroxide masterbatch; both can shift crosslinking during extrusion, increase melt pressure, and reduce the notched slow crack growth response. Contact with copper salts, some transition metal oxides, and strong oxidisers should also be avoided because these can consume the antioxidant package and lower OIT. The material is not intended for injection-moulded fittings requiring spiral mould fill; for such parts, a high-flow HDPE or PE100 compound with melt flow above 1.0 g/10 min is normally specified.
Substitution of GF7750M2 for a PE80 grade changes the pressure rating and wall thickness calculation under ISO 4427-1. Using the standard service design coefficients, a PE100 pipe has a design stress of 8.0 MPa, whereas a PE80 pipe has 6.3 MPa. For a 110 mm outside diameter pipe rated at 16 bar, PE100 SDR11 gives a wall thickness of 10.0 mm; PE80 requires SDR9 with a wall thickness of 12.2 mm. The difference reduces resin mass per metre and increases internal bore diameter, but the thinner wall reduces pipe stiffness because ring stiffness under ISO 9969 scales with the cube of wall thickness. The installation embedment must therefore be compacted more uniformly, particularly for diameters above 160 mm. In gas distribution, qualification to ISO 4437 includes rapid crack propagation testing; PE100 resins normally show an RCP critical temperature below −10 °C, but published data for GF7750M2 in this specific test configuration is limited.
| Requirement | Standard or regulation | Typical evaluation condition |
|---|---|---|
| PE100 classification | ISO 12162 | Lower predictive limit 10 MPa at 50 years, 20 °C |
| Hydrostatic rupture | ISO 1167-1 | 100 h at 20 °C, 12.4 MPa; 1,000 h at 80 °C, 5.4 MPa |
| Slow crack growth | ISO 13479 | Notched pipe, 80 °C, class hoop stress |
| Oxidative induction time | ISO 11357-6 | 210 °C, O₂, >20 min |
| Water supply pipe systems | ISO 4427-1 | Design stress 8.0 MPa for PE100 |
| Gas distribution pipe systems | ISO 4437 | RCP evaluation per national code |
| EU REACH registration | Regulation (EC) No 1907/2006 | Article 33 communication for SVHCs >0.1 wt% |
| RoHS restricted substances | Directive 2011/65/EU | Annex II limits for Pb, Cd, Hg, Cr(VI), PBB, PBDE |
Batch-to-batch monitoring on a 60 mm single-screw extrusion line with a 25:1 L/D screw and spiral mandrel die should include melt pressure upstream of the breaker plate, melt temperature at the die tip, and wall thickness variation at four quadrants. A pressure shift greater than 15 bar at constant screw speed indicates a possible change in the high-molecular-weight fraction or feed-zone cooling. Melt temperature should be kept below 230 °C for natural resin and below 220 °C for carbon-black variants; above these limits, antioxidant consumption accelerates and the inner pipe surface may exhibit discolouration. The pipe wall should be checked with an ultrasonic gauge at 0°, 90°, 180°, and 270°; circumferential thickness variation above 5% can create stress concentrations during hydrostatic testing. For potable water service, the final pipe should be sampled and tested according to national hygiene standards, and the processor should verify that the antioxidant, carbon black, and processing aid packages are covered under the relevant EU or GB food-contact and drinking-water approvals.