| HS Code | 260306 |
| Meltflowrate | 23 g/10 min |
| Meltflowratecondition | 190 °C / 2.16 kg |
| Density | 0.950 g/cm³ |
| Tensileyieldstrength | ≥25 MPa |
| Elongationatbreak | ≥500% |
| Flexuralmodulus | ≥1000 MPa |
| Notchedizodimpactstrength | ≥5 kJ/m² at 23 °C |
| Vicatsofteningtemperature | ≥120 °C |
| Heatdeflectiontemperature | ≥70 °C |
| Meltingpoint | 130-135 °C |
| Hardnessshored | 60-65 |
| Waterabsorption | <0.01% |
| Crystallinity | 70-80% |
| Molecularweightdistribution | Narrow |
| Dielectricconstant | 2.3 |
| Volumeresistivity | >10^16 Ω·cm |
| Form | Pellets |
| Color | Natural |
| Processingmethod | Injection molding |
As an accredited ZPC (Zhejiang Petroleum & Chemical) HDPE 23050 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | ZPC HDPE 23050 typically packed in 25 kg polyethylene-lined woven bags, 40 bags per 1,000 kg pallet. |
| Container Loading (20′ FCL) | 20′ FCL container loading of ZPC HDPE 23050: 25 kg bags, palletized, shrink-wrapped, and securely stowed for safe ocean freight. |
| Shipping | ZPC (Zhejiang Petroleum & Chemical) HDPE 23050 is shipped as a non-hazardous high-density polyethylene resin in 25 kg PE bags or 500–1000 kg jumbo bags, palletized, stretch-wrapped, and loaded into 20' containers. Store cool, dry, ventilated, away from sunlight, heat, moisture, and contamination; handle carefully, avoid punctures and static buildup. |
| Storage | Store ZPC HDPE 23050 in a cool, dry, well-ventilated warehouse. Keep packaging sealed, palletized, and off the floor. Protect from direct sunlight, rain, moisture, heat, open flames, and contaminants. Avoid excessive stacking and prolonged UV exposure. Keep away from strong oxidizers. Do not store outdoors. Use first-in, first-out inventory and follow supplier recommendations. |
| Shelf Life | ZPC HDPE 23050 shelf life is typically 24 months when stored cool, dry, sealed, and protected from direct sunlight. |
Compounding of ZPC HDPE 23050 for PE100 pressure pipe service begins with verification of the lot certificate against ISO 1133-1:2022 and ISO 1183-1:2019 because melt mass flow rate and density define the extrusion window and hydrostatic design basis. For high-molecular-weight HDPE resins of this class, the dry blend is prepared in a high-speed mixer at 40–50 °C jacket temperature with 5.0–6.5 wt% of a 40 % carbon black masterbatch to achieve final carbon black concentration of 2.0–2.5 wt%, while the antioxidant package is dosed as a 0.3–0.8 wt% masterbatch rather than as neat powder to avoid screw feeding variation. The blend is conveyed to a single-screw extruder with grooved feed section, L/D 30:1 to 40:1, and a barrier screw feeding a spiral mandrel die. Barrel temperatures are set from 180 °C at the feed throat to 220 °C at the die, with melt temperature held between 190 °C and 220 °C. Vacuum degassing is applied at −0.6 bar to −0.8 bar relative to atmosphere to remove dissolved moisture and low-molecular-weight volatiles; HDPE pellet moisture is kept below 0.03 wt% before extrusion to reduce surface porosity and bubble formation in the pipe wall. Pipe dimensions are controlled by vacuum calibration sleeves at 0.2–0.5 bar differential pressure, and haul-off speed is trimmed against wall thickness sensors with ±0.3 mm tolerance on SDR 11 and SDR 17 water mains. End products include potable water distribution pipes conforming to ISO 4427 and EN 12201, gas distribution pipes under ISO 4437, and industrial slurry transfer lines. Compliance testing follows hydrostatic design basis evaluation according to ISO 9080, slow crack growth resistance under ISO 13479 with notched pipe specimens at 80 °C, and carbon black dispersion according to ISO 18553. The processing boundary is set by the HDPE rheological class: increasing melt temperature above 230 °C for more than 15 min residence time accelerates oxidative chain scission, while melt temperature below 180 °C reduces homogenization and increases the risk of gel formation in the pipe wall. Published data for this specific ZPC grade configuration is limited, so each lot is pre-evaluated at 190 °C with 2.16 kg load before production starts.
| Property | Standard reference | Measurement condition |
|---|---|---|
| Melt mass flow rate | ISO 1133-1:2022 | 190 °C, 2.16 kg |
| Density | ISO 1183-1:2019 | 23 °C, immersion method |
| Oxidative induction time | ISO 11357-6 | 200 °C, oxygen atmosphere |
| Carbon black dispersion | ISO 18553 | microtome film, rating A1–A3 |
| Hydrostatic design basis | ISO 9080 | long-term extrapolation reference curve |
Accumulator-head extrusion blow molding of high-molecular-weight HDPE 23050 into 220 L open-top drums and 1,000 L intermediate bulk container inner bottles is governed by parison sag, swell, and melt strength, not by mold cavity pressure alone. The accumulator shot size is set to 1.15–1.25 times the net part mass to allow pinch-off weld flash and compensate for parison weight variation; excessive shot volume above 1.30 times net mass increases flash pocket thickness and slows pinch weld cooling rate. Head die gap programming is typically nonlinear: the gap closes to 2.5–4.0 mm during initial parison drop, opens to 5.0–8.0 mm at the top-to-middle transition, and closes again before bottom pinch. Melt temperature is controlled between 180 °C and 200 °C, with extruder barrel zones from 170 °C to 200 °C and die temperature 195 °C to 205 °C. Blow air pressure is 6–8 bar for thick-walled drums and 4–6 bar for IBC liners, while mold cooling water is held at 8–15 °C to stabilize surface gloss and reduce residual internal stress. Regrind from trimmed flash and rejected parts is limited to 20–30 wt% in UN-certified packaging because higher fractions degrade notched Izod impact performance and reduce environmental stress crack resistance under ASTM D1693, condition B at 50 °C with 10 % Igepal CO-630. The pinch weld is the failure-critical zone: weld thickness is maintained at 1.5–2.0 mm per side and mold pinch land angle is verified at 10–15° to avoid fold-back defects and internal stress concentrations. End products include UN 1H2 open-head drums with 220 L nominal capacity, closed-head jerry cans with UN 3H1 classification, and 1,000 L IBC inner bottles under UN 31A with full drop testing at −18 °C. The operational boundary is melt-index related: if the melt mass flow rate of a specific lot falls below the resin’s minimum specification, parison sag decreases but die pressure rises; if it exceeds the maximum, wall thickness distribution becomes erratic and weld strength drops. No nylon or EVOH barrier layer is used in single-material HDPE drums, but fluorination of the internal surface may be applied by downstream converters to reduce permeation of hydrocarbon solvents and oxygen-sensitive fill goods.
Flat-die extrusion of ZPC HDPE 23050 into 1.5 mm and 2.0 mm geomembrane liners is set up with a 120–150 mm, L/D 33:1 single-screw extruder feeding a 3,000–4,500 mm wide flat die with adjustable restrictor bars and internal deckles. The polymer is extruded at melt temperature 220–240 °C onto a mirror-polished three-roll stack, with roll temperatures 70–90 °C and roll gap 1.45–1.95 mm for a 1.5 mm sheet; thickness is measured by beta-gauge or X-ray sensors with ±5 % variation limits. Carbon black concentration is maintained at 2.0–2.5 wt% for ultraviolet stabilization, and the formulation includes 0.05–0.15 wt% hindered amine light stabilizer and 0.05–0.10 wt% phosphite processing stabilizer. Winding tension is kept below 20 N/mm of sheet width to avoid neck-in and residual stress that later forms buckling at the liner toe or seam separation during deployment. Geomembrane sheets from high-molecular-weight HDPE of this class are specified for landfill capping and base lining, mining heap leach pads, ash pond liners, and aquaculture tanks. The material is tested for density, tensile yield and break elongation according to ISO 527-3, tear resistance via ASTM D1004, puncture resistance via ASTM D4833, and oxidative induction time via ISO 11357-6. Stress crack resistance is evaluated under ASTM D5397 single point notched constant tensile load at 50 °C in 10 % Igepal solution. The operational boundary is temperature-related: continuous service above 60 °C reduces antioxidant lifetime and increases susceptibility to environmental stress cracking, and contact with concentrated nitric acid above 25 % at 40 °C is outside the chemical resistance window of HDPE. A production-scale failure commonly observed is edge bead thickness deviation above +10 %, which creates high spots at welded seams; therefore edge trim is removed in-line and passed to regrind at 10–20 wt% in the same extrusion lot, provided the regrind is dried and sieved to avoid gel contamination.
Twisted rope and fishing net yarns made from ZPC HDPE 23050 require monofilament extrusion through a 45–90 mm single-screw extruder with L/D 30:1 and a spinneret plate carrying 80–240 circular holes of 0.6–1.2 mm diameter. The melt is extruded at 210–230 °C into a water quench bath held at 25–35 °C; water temperature above 40 °C slows skin solidification and produces oval cross-sections, while water below 10 °C increases internal void formation and draw-line breaks at the godet stands. Primary godets run at 8–15 m/min, followed by a hot water or hot air draw oven at 80–100 °C and a second-stage draw ratio of 8:1–12:1. Drawing at ratios below 7:1 leaves undrawn core material that reduces tenacity and increases creep under load, whereas ratios above 13:1 create fibrillation and surface cracks that weaken knot strength. Annealing is carried out at 85–100 °C for 2–5 s to shrink the oriented structure by 6–10 % before winding, which stabilizes linear density and reduces spool memory. The formulation includes 0.3–0.6 wt% UV HALS masterbatch and 0.1–0.3 wt% processing aid; blue or green pigment masterbatch is added at 0.5–1.5 wt% for species-specific net visibility or UV screening. Finished monofilament is tested for linear density under ISO 1805, tensile breaking load under ISO 1806, and knot breaking load under ISO 1807. End products include seine nets, trawl nets, mooring hawsers, agricultural trellis twine, and insect barrier screens. The processing boundary is rheological: high-molecular-weight HDPE of this class generates melt pressure of 15–25 MPa before the spinneret; if pressure exceeds 30 MPa, screen pack or spinneret plate replacement is required to avoid localized heat generation and gel-spot defects. Batch-to-batch variation in antioxidant level changes the oxidation onset temperature measured by ISO 11357-6, so incoming lots are preferably pre-screened at 200 °C before monofilament production begins.
Extruded HDPE 23050 sheet for butt-welded chemical storage tanks and scrubber bodies is produced in thicknesses from 3 mm to 20 mm on a flat-die line with L/D 33:1 extruder and vacuum-calibrated roll stack. The sheet is cut, routed, and butt-fused using heater plate welding according to DVS 2207-4, with weld pressure 0.15–0.25 N/mm² and heater plate temperature 200–220 °C. Extrusion welding rods from the same virgin HDPE 23050 compound are spooled after cooling below 45 °C, because spooling warm rod deforms the round cross-section and creates surface oxidation that reduces weld tensile strength and creates microporosity along the weld bead. Weld seams are tested with bend tests and tensile impact, and the fabricated tank is inspected by spark testing with 10–30 kV to detect pinholes and capillary channels. The formulation omits post-consumer recyclate in chemical service; internal regrind from edge trim is limited to 15–25 wt% because excessive regrind narrows the melt flow window and lowers environmental stress crack resistance after long exposure to tank contents. End products include rectangular pickling tanks, electroplating rinse vessels, scrubber housings, and water treatment dosing tanks. Chemical resistance follows ISO/TR 10358 and DVS 2207-4; the material is suitable for dilute mineral acids, alkalis, and salt solutions up to 40 °C, but not for strong oxidizing acids above 25 %, aromatic solvents, or chlorinated hydrocarbons above 40 °C. The operational boundary is thermal expansion: a 10 mm sheet expands approximately 1.2 mm/m per 10 °C temperature rise, so welded tank walls require expansion provision when the design temperature exceeds 50 °C. Published data for this specific ZPC grade configuration is limited; fabricators routinely verify weld factor by destructive testing of the first panel junction and compare the result with the sheet tensile yield value under ISO 527-3.
Multilayer automotive fuel tank shells from high-molecular-weight HDPE 23050 are produced on six-layer coextrusion blow molding machines in which virgin HDPE forms the inner and outer layers, EVOH forms the hydrocarbon barrier, and regrind is encapsulated between barrier and outer layers. Outer layer compound is loaded with conductive carbon black to achieve surface resistivity below 109 Ω/sq per SAE J2260 or IEC 61340-5-1 to avoid static discharge during refueling. The inner layer is unpigmented virgin HDPE with high melt strength and a melt mass flow rate in the same class as ZPC HDPE 23050; barrier layer thickness is 2–4 % of total wall thickness, and regrind layer content is limited to 30–50 wt% of total shell mass. Parison programming is linked to blow mold geometry to maintain wall thickness from 3 mm at the pinch flange to 6 mm at the insert zones. Melt temperature is controlled at 200–230 °C for HDPE layers and 190–210 °C for EVOH, with die head temperature 205–225 °C. Blow air pressure is 8–12 bar, and mold temperature is held at 15–25 °C. The fuel tank shell is tested for impact resistance after conditioning at −40 °C, permeation under CARB LEV III or Euro VI evaporative emission limits, and pressure-cycle durability. The processing boundary is the EVOH layer: residence time in the die head above 30 min at 220 °C causes EVOH degradation and black specks in the barrier layer. HDPE 23050 is not used as the sole fuel tank material without a barrier layer when permeation limits are below 2 g/m²/day. End products include high-density polyethylene fuel tanks for passenger cars, commercial vehicles, and off-road machinery.
Competitive ZPC (Zhejiang Petroleum & Chemical) HDPE 23050 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
ZPC (Zhejiang Petroleum & Chemical) HDPE 23050 is a bimodal high-density polyethylene resin classified as PE100 under ISO 12162. Its melt mass-flow rate measured at 190 °C with a 5.0 kg load according to ISO 1133-1:2022 is typically 0.23 g/10 min, and its density according to ISO 1183-1:2019 is approximately 0.950 g/cm³. The grade is directed at solid-wall pressure pipe extrusion for municipal water supply and industrial fluid transport where the finished pipe is qualified under ISO 4427, ISO 4437, or EN 12201. The bimodal molecular weight distribution separates the resin from general-purpose HDPE grades by combining a low-molecular-weight fraction for processability with a high-molecular-weight, comonomer-modified fraction for long-term creep and slow crack growth resistance.
The following batch-release profile characterises ZPC HDPE 23050 under standardised laboratory conditions. The values do not supersede lot-specific certificates of analysis, but they establish the density and flow class that govern downstream drying, screw selection, and die pressure behaviour.
| Property | Test method | Typical value |
|---|---|---|
| Melt mass-flow rate, 190 °C / 5.0 kg | ISO 1133-1:2022 | 0.23 g/10 min |
| Density, 23 °C | ISO 1183-1:2019 | 0.950 g/cm³ |
| Tensile yield stress | ISO 527-2:2012 | 23 MPa |
| Elongation at break | ISO 527-2:2012 | >600% |
| Notched pipe slow crack growth, 80 °C / 4.6 MPa | ISO 13479:2022 | ≥500 h |
| Hydrostatic strength classification, 20 °C / 50 years | ISO 9080, ISO 12162 | PE100, MRS 10 MPa |
The 0.950 g/cm³ density and 0.23 g/10 min melt flow rate place the grade in the high-molecular-weight pipe-grade window. These parameters alone do not define PE100 compliance; the PE100 classification is assigned through long-term hydrostatic strength regression and lower prediction limit analysis under ISO 9080. The minimum required strength of 10 MPa permits a design stress of 8.0 MPa at 20 °C when a service coefficient of 1.25 is applied under ISO 12162 assumptions.
In molecular terms, the bimodal architecture of ZPC HDPE 23050 consists of a lower-molecular-weight homopolymer fraction that controls melt transport and drawability, and a higher-molecular-weight α-olefin copolymer fraction that increases tie-molecule connectivity between crystalline lamellae. This architecture shifts the ductile-to-brittle transition on pipe stress-rupture curves toward longer failure times under sustained hoop stress. Unlike unimodal HDPE of equivalent density, the grade retains processability because the low-molecular-weight fraction acts as an internal processing aid during melting and metering.
Pipe extrusion lines for ZPC HDPE 23050 typically employ grooved-feed, single-screw extruders with an L/D ratio of 30:1 to 36:1 and spiral mandrel dies. The grooved feed zone generates high pre-melt pressure and prevents pellet slip because the high-molecular-weight fraction cannot be conveyed reliably on smooth-bore, flood-fed screws without excessive melt-temperature rise. Extrusion blow-moulding grades of similar density but narrower molecular weight distribution can be run on smooth-bore screws with shallower compression ratios. On grooved-feed equipment, barrel set temperatures are commonly held between 190 °C and 220 °C, with the die head set 5–15 °C higher. Melt temperatures above 235 °C should be avoided because shear heating in the metering zone can degrade the high-molecular-weight fraction and reduce notched slow crack growth resistance measured later under ISO 13479:2022.
At screw speeds above 90 min⁻¹ on a 75 mm grooved-feed extruder, barrel pressure can exceed 350 bar. Under these conditions, melt temperature may rise by 3–8 °C per 10 min⁻¹ increase in screw speed, depending on screw geometry and back pressure. The use of a melt pump before the die is common on large-diameter pipe lines to reduce pulsing and maintain wall thickness tolerance. Pre-drying is not required under normal indoor storage conditions, but resin stored at relative humidity above 60% or exposed to rain should be dried at 80 °C for 2 h to prevent surface pinholes and internal voids in the pipe wall.
Slow crack growth resistance in pipe form is evaluated under ISO 13479:2022, in which a notched pipe specimen is subjected to 80 °C water and 4.6 MPa hoop stress. PE100 resins generally require failure times of at least 500 h under this test. ZPC HDPE 23050 is positioned for installations where point loads from rock impingement, thermal contraction, or inadequate bedding impose sustained tensile stress at crack tips. Under ISO 1167 hydrostatic testing, PE100 compounds are expected to resist ductile deformation and brittle fracture within the extrapolated 50-year service envelope defined by ISO 9080. For high-chlorine potable water, hydrocarbon condensates, or oxidising process fluids, case-specific chemical resistance testing is required because rapid crack propagation and slow crack growth accelerate in aggressive environments.
Relative to PE80 pipe grades, ZPC HDPE 23050 provides higher minimum required strength and potential wall-thickness reduction at the same nominal pressure rating. However, that strength comes with higher melt viscosity and a narrower processing window; substitution of a PE80 grade with PE100 is not a direct drop-in change on an existing screw geometry without verifying melt temperature, die pressure, and output stability.
Zone set-point requirements vary with extruder diameter and screw geometry. On a 60–75 mm grooved-feed extruder with 30:1 L/D, indicative set-points are: feed 180–190 °C, compression 190–200 °C, metering 200–215 °C, and die 210–225 °C. Melt temperature should be measured with an immersion probe before the melt pump; a reading above 230 °C indicates excessive screw speed, worn screw elements, or insufficient back pressure. For pipe outside diameters above 160 mm, die head pressure typically ranges between 200 bar and 350 bar depending on die gap and throughput. At die head pressure above 400 bar, the risk of melt fracture and die-lip plating increases, and screw speed should be reduced or die temperature raised in 5 °C increments.
Vacuum calibration tank temperatures are normally maintained between 15 °C and 25 °C to solidify the pipe wall without excessive thermal stress. A high outer-surface cooling rate can produce residual stresses that reduce slow crack growth resistance; multi-zone cooling with graduated water temperatures is therefore preferred over single-point quenching. For black pipe formulations, final carbon black content should be 2.0–2.5% by weight according to ISO 6964. Carbon black dispersion should be verified by ISO 18553, because agglomerates above 0.1 mm reduce slow crack growth resistance and create stress concentrators in the pipe wall.
Compared with general-purpose injection-grade HDPE with melt flow rates of 7–20 g/10 min at 2.16 kg, ZPC HDPE 23050 exhibits substantially higher melt viscosity and a narrower processing window. It is not suitable for thin-wall injection moulding where fill pressure would exceed clamp force capacity on machines below 1,000 kN. Compared with blown-film HDPE, the resin is not optimised for bubble stability at high blow-up ratios; its molecular weight distribution is tuned for thick-walled annular flow in pipe sizing. Compared with extrusion blow-moulding grades such as HDPE 5502, ZPC HDPE 23050 has a lower standard-load melt flow rate and a lower density, but direct comparison requires testing at identical load and temperature.
| Parameter | ZPC HDPE 23050 | General-purpose injection HDPE | Extrusion blow moulding HDPE |
|---|---|---|---|
| Melt flow rate | 0.23 g/10 min at 5.0 kg | 7–20 g/10 min at 2.16 kg | 0.2–0.4 g/10 min at 2.16 kg |
| Density | 0.950 g/cm³ | 0.950–0.960 g/cm³ | 0.954–0.956 g/cm³ |
| Primary processing | Pipe extrusion | Injection moulding | Extrusion blow moulding |
| Notched slow crack growth | ≥500 h | Lower; not PE100 | Moderate; not typically PE100 |
Regulatory qualification for potable water and gas service belongs to the pipe converter, not the resin supplier. The grade should be evaluated in final pipe form under EN 12201, ISO 4427, ISO 4437, or applicable national standards. In regrind operations, recycled content above 20% can reduce slow crack growth resistance and hydrostatic durability; any regrind blend must be revalidated in pipe form. The published data for ZPC HDPE 23050 in chlorinated potable water at service temperatures above 40 °C is limited; long-term field validation is recommended before projecting service life beyond the standard design envelope.