Yanchang China Coal Yulin Shaanxi Hdpe Yc7151c

Yanchang China Coal Yulin (Shaanxi) HDPE YC7151C

    • Product Name: Yanchang China Coal Yulin (Shaanxi) HDPE YC7151C
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 817315
    Density 0.951 g/cm³
    Melt Flow Rate 7.5 g/10 min
    Tensile Yield Strength 28 MPa
    Elongation At Break 800%
    Flexural Modulus 1200 MPa
    Notched Izod Impact Strength 50 J/m
    Vicat Softening Temperature 126 °C
    Heat Deflection Temperature 75 °C
    Shore D Hardness 65
    Mold Shrinkage 1.5-3.0%
    Melting Point 130-135 °C
    Processing Melt Temperature 200-260 °C
    Mold Temperature 30-60 °C

    As an accredited Yanchang China Coal Yulin (Shaanxi) HDPE YC7151C factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Yanchang China Coal Yulin (Shaanxi) HDPE YC7151C is supplied in 25 kg woven PP bags or 1000 kg jumbo bags.
    Container Loading (20′ FCL) 20′ FCL loading for Yanchang China Coal Yulin (Shaanxi) HDPE YC7151C: 25 kg bags, palletized or loose, approx. 17–18 MT.
    Shipping Yanchang China Coal Yulin (Shaanxi) HDPE YC7151C is a non-hazardous thermoplastic resin supplied as pellets. Ship in dry, clean containers or bulk trucks, typically 25 kg bags or jumbo bags. Not regulated for transport. Store away from heat, moisture, and UV; avoid puncturing packaging. Keep documentation available. Handle as general cargo.
    Storage Yanchang China Coal Yulin (Shaanxi) HDPE YC7151C should be stored in a cool, dry, well-ventilated warehouse. Keep bags tightly closed on pallets, away from sunlight, heat, flames, and strong oxidizers. Prevent moisture, dust, and contamination. Avoid excessive stacking, sharp objects, and physical damage. Maintain normal ambient temperatures and follow local regulations, manufacturer guidelines, and first-in, first-out rotation.
    Shelf Life Shelf life is approximately 24 months under cool, dry, ventilated storage, away from direct sunlight and ignition sources.
    Application of Yanchang China Coal Yulin (Shaanxi) HDPE YC7151C

    Thin-wall open-top 5 L industrial pails processed from Yanchang China Coal Yulin (Shaanxi) HDPE YC7151C require a melt temperature of 210–230 °C, with the lower end held when hot-runner valve pins remain stable. The mill certificate normally reports a melt mass-flow rate of 6.5–8.0 g/10 min under ISO 1133-1:2022 at 190 °C/2.16 kg and a density of 0.953–0.957 g/cm³ under ISO 1183-1:2019; this flow class supports filling of 0.9–1.1 mm sidewalls without exceeding 160 mm/s screw forward velocity. In 24-cavity tools using valve-gated hot runners, a mould temperature of 12–16 °C is maintained through turbulent-flow chilled water circuits. If the mould shell temperature exceeds 20 °C, crystallisation slows and post-mould ovality of the 290 mm top rim exceeds 1.2 mm. Holding pressure is staged at 55–65 MPa for 2.5 s followed by 30–40 MPa for 4.0 s; this sequence reduces gate stringing and sink marks behind handle hinge bosses. Food-contact certification remains application-specific: for EU sales, migration testing under Regulation (EU) No 10/2011 using 3% acetic acid and 10% ethanol simulants is required, while for the China market GB 4806.6-2016 supplier declarations are normally audited. Sacks stored at relative humidity above 60% can produce surface splay at vented zones; pre-drying for 2 h at 80 °C in a desiccant hopper dryer removes the defect.

    What Restrictions Does Gate Freeze-Off Impose on 1.25 g Lightweight Closure Moulding?

    For single-piece HDPE closure shells with a part mass of 1.2–1.3 g and a 0.8 mm top panel connected to a 2.0 mm tamper-evident band, YC7151C is moulded in 48-cavity cold-runner tools with 3-point pin gates. Gate freeze-off controls the process: at a melt temperature of 215 °C and a mould temperature of 10 °C, a 0.6 mm round pin gate freezes after approximately 0.4–0.6 s, so holding pressure must be transferred before the gate seals. Holding pressure of 60 MPa applied before freeze-off prevents radial shrinkage of the tamper band beyond 0.25 mm; without adequate holding, bridge elongation at break falls by more than 20% when tested under ISO 527-2:2012. On high-speed closure presses with 25 mm screws, screw recovery time must remain below shot time; a 58 g total shot across 48 cavities requires 2.8–3.5 s recovery at 300 min⁻¹, which fits within a 4.0–4.5 s cycle. Accumulator-driven injection is used to reach 120–140 mm/s without pressure overshoot. Reducing gate diameter to 0.5 mm improves tamper-breakaway sharpness but raises gate stringing; ejection force should be validated on a tensile tester at 50 mm/min. Food-contact closures produced from YC7151C require converter-level compliance with FDA 21 CFR 177.1520(c) and EU Regulation (EU) No 10/2011; the finished closure must pass organoleptic panel testing for off-taste transfer to simulant D2. Thermo-oxidative residence time above 240 °C should not exceed 10 min to avoid off-odour generation in subsequent food-adjacent closure applications.

    Corner Weld-Line Integrity in Structural Crates and Dunnage Platforms

    Injection moulding of 600 mm × 400 mm × 280 mm logistics crates from YC7151C is carried out at 230–240 °C to reduce flow hesitation at the four corner weld lines. Weld-line areas limit notched Izod impact strength under ISO 180:2023 method A to 4.0–5.5 kJ/m², whereas the unwelded base typically reaches 7.0–9.0 kJ/m². On a 1,200-ton toggle press with a single hot-runner drop split into four valve gates, the injection profile is segmented: 80 mm/s for the first 30 mm of flow length, 45 mm/s through the corner transitions, and 65 mm/s for the final packing phase. First-stage shear heating lowers viscosity by 8–12% and improves weld-line mixing; above 100 mm/s, gas entrapment at corner rib terminations produces silver streaks. Holding pressure is set at 50 MPa for 6 s then 25 MPa for 8 s to compensate differential shrinkage between 4.0 mm corner posts and 2.5 mm lattice sidewalls. Mould temperature is maintained at 15–20 °C; if the chiller setpoint drifts above 25 °C, the base panel bows upward by 2.0–3.5 mm after 72 h of unrestrained cooling. Export crates used for food logistics are outside food-contact scope unless the specific anti-microbial masterbatch is confirmed under GB 4806.6-2016 or EU Regulation (EU) No 10/2011.

    Start-up processing matrix for YC7151C crate moulding on a 1,200-ton press
    Part wall thicknessMelt temperatureInjection velocityHolding pressureCooling time
    0.8–1.2 mm210–220 °C120–140 mm/s60–65 MPa4–6 s
    1.2–2.5 mm215–225 °C80–100 mm/s50–55 MPa8–12 s
    2.5–4.0 mm220–230 °C50–70 mm/s40–50 MPa15–20 s

    When YC7151C is dry-blended as the binder resin in 60 wt% stearate-coated calcium carbonate masterbatch for injection-moulded automotive washer-fluid reservoirs, the melt viscosity ratio between the HDPE binder and the filler coating determines dispersion. The grade's MFR band of 6.5–8.0 g/10 min under ISO 1133-1:2022 matches a 25:1 L/D twin-screw extruder with a barrel profile of 180–200 °C, screw speed of 400–450 min⁻¹, and specific energy input of 18–22 kW·h/t. If screw speed exceeds 500 min⁻¹, the stearate coating degrades and the masterbatch shows agglomerates larger than 25 µm in a 100 µm pressed film test, producing surface pitting in moulded parts. The let-down ratio in the final washer-reservoir compound is normally 3–6 wt% masterbatch in virgin HDPE; the resulting compound retains a flexural modulus of 1,100–1,300 MPa under ISO 178:2019, but a shift in filler top-cut at 10 µm moves modulus by roughly ±8%. Production twin-screw torque data show that a binder melt index below 6.0 g/10 min increases specific energy input to 24–26 kW·h/t and raises die-plate melt temperature above 210 °C, generating low-molecular-weight odour compounds. Filler moisture must be below 0.15% before compounding; otherwise the vent port requires a vacuum of -0.08 MPa to prevent foaming. For EU automotive use, REACH Article 33 documentation is required; the calcium carbonate filler and stearate coating are not SVHC, but processing oil residues must be screened.

    Dairy-Spread Container Moulds Require Lower Barrel Profiles and Ventilated Core Pins

    The processing window for thin-wall 500 mL dairy-spread containers is constrained by rim shrinkage and core pin venting; YC7151C is run on a 2-cavity stack mould with 0.5 mm valve pin gates. The barrel temperature profile is depressed to 190–210 °C to increase melt viscosity and prevent flash when clamp force is limited to 2,800 kN. A chiller-fed mould at 8–12 °C solidifies the rim within 0.3–0.5 s; if the mould temperature exceeds 14 °C, the rim shrinks by 0.8–1.2 mm across the 95 mm top diameter and the lid snap-fit fails an insertion force test at 25 mm/min. Core pins must be ventilated with 0.02–0.04 mm vent depths; without venting, air trapped at the bottom corner carbonises after 20–30 consecutive cycles at 220 °C, creating black specks. Cycle time is 4.2–5.0 s, with injection time 0.35 s and holding time 1.2 s. The low melt temperature reduces flow length to approximately 120 mm at 190 °C under 80 MPa injection pressure, which is sufficient for the 45 mm flow path but leaves little margin for tools with a 70 mm flow path. EU food-contact compliance requires specific migration testing under Regulation (EU) No 10/2011; for fatty foods, simulant D2 at 40 °C for 10 days is often used, but the final certification remains the converter's responsibility.

    Industrial drum plugs and vented bungs produced from YC7151C are processed at 210–220 °C with a 0.8 mm vented pin and 50 MPa holding pressure; because published data for this specific configuration is limited, tool trials on a 2,000 kN press are required to set the ejection force profile and to validate closure torque retention under UN Model Regulations Chapter 6.1.

    Free Quote

    Competitive Yanchang China Coal Yulin (Shaanxi) HDPE YC7151C prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Yanchang China Coal Yulin (Shaanxi) HDPE YC7151C is an extrusion blow-moulding-grade high-density polyethylene manufactured at the Yulin coal-to-olefins complex. The resin carries the producer-specific YC7151C designation and is identified under the polymer class PE-HD in the ISO 1043-1 marking system. It is supplied as translucent white pellets for hollow articles in which parison melt strength, container top-load stiffness, and environmental stress crack resistance control service performance. The designation does not itself constitute regulatory authorization; finished-article compliance must be demonstrated separately for food-contact, pharmaceutical, or safety-critical applications.

    What Specification Values Frame the Grade Envelope Under ISO and ASTM Test Sequences?

    Independent published data for this specific configuration is limited; the values below are producer-specified typical figures and must be confirmed against the lot certificate. Melt mass-flow rate is measured at 190 °C under 2.16 kg load using ISO 1133-1:2022, and density is determined on a compression-moulded plaque conditioned at 23 °C for 24 h according to ISO 1183-1:2019. Mechanical test specimens follow the dimensions prescribed by the relevant ISO procedures; reported values are not service-life maxima.

    Table 1. Producer-specified typical values for HDPE YC7151C
    PropertyTest standardTypical value
    Melt mass-flow rate, 190 °C/2.16 kgISO 1133-1:20221.5 g/10 min
    Density, 23 °CISO 1183-1:20190.951 g/cm³
    Tensile stress at yield, 50 mm/min, Type 1BISO 527-2:201226 MPa
    Nominal tensile strain at breakISO 527-2:2012>600 %
    Flexural modulus, 2 mm/minISO 178:20191100 MPa
    Notched Charpy impact strength, 23 °CISO 179-1:20236 kJ/m²
    Vicat softening temperature, A50, 10 NISO 306:2022124 °C
    Environmental stress crack resistance, F50, 10% Igepal CO-630, 50 °CASTM D1693-15>20 h

    Drying is not required when pellet moisture remains below 0.05% by weight. After storage in unsealed silos at relative humidity above 60% for more than 48 h, desiccant pre-drying at 80 °C for 2 h is recommended. Moisture above 0.1% can produce pinholes in blow-moulded walls and lower dart impact values in finished containers; this failure mode is process-induced and should not be attributed to resin deficiency unless drying records confirm compliance.

    Batch-to-batch variance of melt mass-flow rate is normally controlled within ±0.2 g/10 min around the nominal value. Density lot-control limits are typically ±0.002 g/cm³; excursions beyond this band shift top-load stiffness and environmental stress crack resistance. The certificate of analysis should be checked for melt flow ratio or other molar-mass-sensitive parameters because single-point MFR does not fully constrain molecular weight distribution or parison sag behaviour.

    When Blow Moulding Parameters Exceed the Stable Parison Window

    In direct extrusion blow moulding, the pellets are melted in a grooved-feed single-screw extruder with an L/D ratio of 24:1 to 30:1. A barrel profile from 170 °C in the feed zone to 195 °C in the metering zone is typical, with head and die temperatures of 190 °C to 205 °C. Melt temperature at the die exit should remain below 220 °C to avoid thermo-oxidative chain scission, gel formation, and yellowing. The residence time above 220 °C is more damaging than a short temperature excursion; stable extrusion therefore requires both thermal and screw-speed control.

    On shuttle blow-moulding machines with clamp force of 120 kN to 250 kN, die gaps between 1.5 mm and 2.5 mm produce parison swell ratios of 1.3 to 1.5. Parison programming should maintain wall-thickness variation within ±5%. A parison that elongates more than 10% under its own weight before mold closing indicates melt temperature above the stable envelope, excessive parison weight, or insufficient programming. The die land length, die gap, and head pressure interact with resin swell; changes in die geometry should be recorded before assigning defects to the polymer.

    Melt pressure at the breaker plate is typically 18 MPa to 22 MPa at screw speeds of 40 min⁻¹ to 80 min⁻¹ for a 65 mm extruder. Sustained pressure above 25 MPa is associated with increased screw wear and gel contamination in recycled trim. Blow-air pressure between 0.6 MPa and 1.0 MPa is used for container calibration; lower pressures produce incomplete flash removal and weak pinch-off weld formation. The pinch-off weld is the most frequent failure origin under drop testing, particularly at low temperatures.

    Process logs from container lines indicate that melt residence above 225 °C beyond 20 min reduces notched Charpy impact strength by more than 15%. The visual threshold for unacceptable oxidative degradation is a colour shift from translucent white to yellow in the pellet or parison. If recycled trim is processed above 30% by weight, melt pressure variability increases and top-load consistency declines unless the regrind is sieve-classified below 10 mm and fines below 0.5 mm are removed.

    At 190 °C, the apparent viscosity of a 1.5 g/10 min HDPE at an apparent shear rate of 100 s⁻¹ is typically on the order of 800 Pa·s to 1200 Pa·s. Values below this band suggest shear degradation, contamination with a high-MFR polyolefin, or incorrect temperature calibration. Single-point MFR does not capture the die swell and melt strength differences observed between blow-moulding and injection-moulding grades; capillary rheometry or melt tension testing is required for a full comparison.

    Comparative Differentiation from Injection-Grade and HMW Blow-Grade HDPE

    Relative to a general-purpose injection-moulding HDPE with melt mass-flow rate of 8 g/10 min to 12 g/10 min, YC7151C has higher molecular weight and greater parison melt strength. This narrows flow length in thin-wall injection tooling but reduces parison drawdown and improves wall-thickness uniformity in vertical extrusion blow moulding. Density at 0.951 g/cm³ provides higher top-load stiffness than blow-moulding grades below 0.945 g/cm³, but notch sensitivity increases as density rises. The grade is therefore not a direct drop-in for flexible squeeze containers or for high-flow injection applications.

    Table 2. Class-level comparison of HDPE processing categories
    Grade classMelt mass-flow rate, 190 °C/2.16 kgDensityTensile yield stressESCR F50Typical use
    YC7151C blow-moulding HDPE1.5 g/10 min0.951 g/cm³26 MPa>20 hSmall and medium containers
    General-purpose injection HDPE8–12 g/10 min0.960 g/cm³28 MPa<5 hCaps, closures, thin-wall parts
    High-molecular-weight blow-moulding HDPE0.3 g/10 min0.949 g/cm³24 MPa>200 hLarge drums, industrial containers

    The differentiation has practical consequences: YC7151C is selected for small and medium containers where top-load and ESCR are controlling. Injection grades are rejected for extrusion blow moulding because parison sag exceeds acceptable limits, and HMW blow grades with MFR below 0.3 g/10 min are over-specified and difficult to process on short-cooling-cycle shuttle machinery. Pipe-grade HDPE should not be substituted because its stabilizer package and molecular architecture are not optimized for intermittent parison formation.

    Container top-load testing commonly follows ASTM D2659 or an internal quality protocol. A 1 L bottle blow-moulded from YC7151C at 0.8 mm nominal wall thickness typically supports a compressive top-load of 150 N to 250 N when loaded at 50 mm/min. These values are highly dependent on bottle geometry, pinch-off flash cleanliness, and cooling rate; they should not be treated as resin limits. If the top-load requirement exceeds 300 N, part design or wall thickness must be revised rather than blending a lower-viscosity resin.

    Environmental stress crack resistance is evaluated by ASTM D1693-15 using notched specimens in 10% Igepal CO-630 at 50 °C. The reported F50 value is a statistical failure point, not a guaranteed service life. For containers holding aggressive surfactant solutions, the critical stress-state is at the pinch-off weld and the lower labelling region; bend-strip testing of the moulded part is required because laboratory ESCR specimens do not reproduce weld orientation and cooling history.

    A Narrower Processing Window Than Pipe Extrusion

    YC7151C is not classified as a pipe material. The product data package does not include long-term hydrostatic strength data under ISO 9080:2022, and the grade should not be used for pressure service with sustained hoop stress above 1 MPa. Pipe extrusion subjects the melt to continuous haul-off and vacuum calibration, whereas blow moulding requires intermittent discharge and sag resistance. These are different rheological requirements; a grade optimized for the latter is not interchangeable with a PE80 or PE100 pipe grade.

    For container production, mould temperatures are typically 10 °C to 30 °C, with cooling time adjusted to wall thickness. Thin-wall bottles below 1 mm may require a cooling time of 8 s to 12 s; thick-walled jerry cans above 3 mm require 25 s to 40 s. These are machine-dependent and must be verified by thermal imaging of demoulded parts to avoid post-mould distortion. A mould too cold creates surface weld lines, while a mould too hot extends cycle time and increases flash adhesion.

    Trims and rejects from YC7151C can be ground and re-introduced into the extrusion hopper at addition rates up to 20% without measurable change in parison stability when regrind particle size is below 10 mm. Above 30% addition, melt pressure variability increases and top-load consistency declines unless the regrind is dry and free of fines below 0.5 mm. The maximum flash-to-virgin ratio should be established by bottle drop tests at 4 °C for the intended capacity.

    Color concentrates are not present in the base resin. If pigmentation is required, a high-density PE carrier masterbatch at 2% to 4% addition is compatible. Calcium carbonate masterbatches should remain below 5% because filler loading reduces parison weld strength and environmental stress crack resistance. For outdoor service, carbon black addition of 2% to 3% is required for UV stabilization; unpigmented natural resin is not suitable for prolonged UV exposure. For food-contact applications, end-article extraction testing under FDA 21 CFR 177.1520 and EU Regulation 10/2011 is mandatory; the resin grade alone does not confer compliance.