| HS Code | 161497 |
| Density | 0.955 g/cm³ |
| Melt Flow Rate | 0.35 g/10 min (190°C/2.16 kg) |
| Tensile Yield Strength | ≥25 MPa |
| Tensile Break Strength | ≥20 MPa |
| Elongation At Break | ≥500% |
| Flexural Modulus | ≥1100 MPa |
| Notched Izod Impact Strength | ≥15 kJ/m² |
| Hardness Shore D | ≥60 |
| Vicat Softening Temperature | ≥120 °C |
| Brittleness Temperature | ≤-70 °C |
| Melting Point | 130-135 °C |
| Heat Deflection Temperature | ≥80 °C |
| Volume Resistivity | ≥1×10^16 Ω·cm |
| Dielectric Constant | 2.3 |
| Water Absorption | ≤0.01% |
| Mold Shrinkage | 1.5-3.0% |
| Environmental Stress Cracking Resistance | ≥1000 h |
| Molecular Weight Distribution | Narrow |
| Ash Content | ≤0.02% |
| Volatile Matter | ≤0.2% |
As an accredited Yanchang China Coal Yulin (Shaanxi) HDPE HD5503S factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Yanchang China Coal Yulin (Shaanxi) HDPE HD5503S packaging: 25 kg net woven bags, palletized and stretch-wrapped for transport. |
| Container Loading (20′ FCL) | 20′ FCL loading: approximately 17 MT HDPE HD5503S in 25 kg bags, typically 680 bags per container. |
| Shipping | Yanchang China Coal Yulin (Shaanxi) HDPE HD5503S is a non-hazardous, solid high-density polyethylene resin. It is shipped in 25 kg bags or jumbo bags, palletized and wrapped, via truck, rail, or container. Store dry and ventilated, away from heat, moisture, and direct sunlight. Keep bags sealed. |
| Storage | Store Yanchang China Coal Yulin (Shaanxi) HDPE HD5503S in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, flames, and strong oxidizers. Keep original bags sealed, palletized, and off the floor. Prevent moisture, dust, and contamination. Avoid prolonged UV exposure and static buildup. Maintain moderate temperature, preferably below 50°C, and follow manufacturer/local safety regulations. Use first-in, first-out stock rotation. |
| Shelf Life | Shelf life: typically 24 months from production when stored cool, dry, well-ventilated, in original unopened packaging, away from direct sunlight. |
In pressure pipe compounding for potable water and fuel gas distribution, Yanchang China Coal Yulin (Shaanxi) HDPE HD5503S is processed as the high-molecular-weight base resin. With a nominal density of 0.955 g/cm³ and an MFR₂.₁₆ of 0.30–0.40 g/10 min measured under ISO 1133-1:2022, the grade requires grooved feed extruder hardware rather than smooth-bore barrel equipment; on a screw with L/D 30:1–36:1 and a barrier mixing section, the melt pressure at the die head is maintained below 350 bar to prevent screen pack deformation and excessive shear heating. For black PE100-type pressure pipe compounds, HD5503S is combined with 5.0–6.25 wt% of a 40% carbon black masterbatch and 0.10–0.25 wt% of a processing stabilizer masterbatch, yielding a final carbon black content of 2.0–2.5 wt% as required by ISO 4427-1:2019 and ISO 4437-1:2024 for black compounds. For blue potable water service, the carbon black masterbatch is replaced by 0.8–1.5 wt% of a blue masterbatch containing phthalocyanine pigments and a hindered amine light stabilizer package; this substitution must not alter the hydrostatic design basis of the compound, which is verified by ISO 9080:2022 and ISO 1167-1:2006 long-term pressure testing. In production, the blended compound is extruded through a pipe die with vacuum calibration at -0.03 to -0.06 MPa and quenched in water baths held at 20–40°C; dimensional control of SDR 11 and SDR 17.6 pipes is monitored by ultrasonic wall-thickness gauges after the haul-off. Typical downstream pipe dimensions range from DN 32 to DN 630, with output rates of 250–400 kg/h on production-scale single-screw pipe lines. The terminal product types include duplex PE100 drinking water mains, municipal gas distribution pipes, and industrial slurry transfer lines. Field data from pipe extrusion lines indicate that the main processing bottleneck is not melt temperature but the grooved feed zone: barrel zone 1 must remain below 160°C to prevent premature melting and pellet bridging, which can reduce throughput by 15–20%. Compliance for potable water includes EN 12201-1:2024, ASTM D3035-20, and ASTM F714-20 where applicable; for fuel gas, ISO 4437-1:2024 governs compound and pipe design. Prior to compounding, bulk storage at RH > 60% requires pre-drying at 80°C for 2 h to keep moisture below 0.05 wt%, otherwise surface microvoids appear in the pipe wall and reduce the 20°C/12.4 MPa/100 h hydrostatic survival probability.
On accumulator-head blow moulding lines, HD5503S is combined with 0–20 wt% in-house regrind from die flash and edge trim; the base resin fraction is therefore 80–100 wt%. For UN-certified black drums, a 1.0–2.0 wt% carbon black masterbatch is added, and where outdoor storage is specified, 0.3–0.5 wt% of a hindered amine light stabilizer masterbatch is introduced. Regrind concentration above 20 wt% raises the melt flow rate and reduces hoop strength consistency, producing parison wall-thickness variation that the accumulator programming cannot fully correct. The production process uses an accumulator-head machine with a clamp force of 80–120 tonnes for 200-L drums; the extruder L/D is typically 24:1–30:1, melt temperature is held at 180–210°C, and the die gap is set at 8–12 mm. Parison programming with 100-point wall-thickness control adjusts the die gap during extrusion to compensate for gravity-driven parison sag; when melt temperature exceeds 215°C, parison drawdown over a 1.6 m length rises above 12%, and top-to-bottom wall thickness deviation exceeds 1.5 mm in the chimb and bottom rim areas. Mould cooling water at 8–12°C is used to freeze the part surface before demoulding, with a total cycle time of 110–150 s for a 200-L tight-head drum. Terminal product types include UN 1H1 tight-head drums, 1H2 open-head drums for high-viscosity chemical pastes, and 1000-L IBC inner bottles. Regulatory compliance for dangerous goods packaging is demonstrated by 49 CFR 178.509 and ADR 6.1.5.2 performance tests, including stack loading, leakproofness, hydraulic pressure, and drop tests at -18°C. A recurrent field failure occurs when regrind is overdried or contaminated with polypropylene closures: PP contamination creates low-viscosity inclusions at 190–210°C and produces pinholes in the pinch-off weld; therefore, separation of closure regrind is mandatory before reprocessing.
A 1.5 mm HDPE geomembrane formulation based on HD5503S is compounded with 2.5–3.5 wt% of a 50% carbon black masterbatch to achieve 2.0–2.5 wt% final carbon black, plus 0.3–0.7 wt% of a hindered amine light stabilizer masterbatch. Calcium carbonate filler is restricted to ≤1.0 wt% because higher filler loadings reduce environmental stress crack resistance and push the compound density above the 0.940–0.960 g/cm³ window accepted by GRI GM13 for HDPE geomembrane. Flat-die sheet extrusion is carried out on a single-screw extruder with L/D 30:1–36:1 and a die width of 2.0–3.2 m; melt temperature is controlled at 200–230°C, and the polished roll stack is held at 70–95°C to set surface gloss and thickness. On-line beta or X-ray backscatter gauges maintain sheet thickness at 1.0–2.5 mm with a tolerance of ±10% per ASTM D5199-12. When melt residence time exceeds 20 min or melt temperature exceeds 230°C, standard oxidative induction time falls below 100 min as measured by ASTM D3895-19; for this reason, screen pack filtration with 60/100/60 mesh packs is changed before each 72 h production run. The extrusion output ranges from 500–850 kg/h depending on die width and roll speed. Terminal products include landfill bottom liners, heap leach pads in copper and gold mining, tailings impoundment liners, and floating covers for manure lagoons. Compliance is assessed against GRI GM13, ASTM D6693-20 for tensile properties, ASTM D5885-06 for high-pressure OIT, and EN 13492:2018 for installation-related performance. An operational incompatibility exists with amine-based antistatic additives, which interfere with the hindered phenol/phosphite antioxidant system and reduce OIT more rapidly than thermal abuse alone; therefore, antistat masterbatches are not used in geomembrane formulations unless specifically validated by ASTM D3895-19 and ASTM D5885-06.
Double-wall corrugated drainage pipe manufacturing imposes a different demand on HD5503S than pressure pipe extrusion: the corrugator freezes the outer wall within seconds, so high melt strength and fast crystallisation are both required. The formulation uses 94.0–95.0 wt% HD5503S with 4.0–5.0 wt% of a 50% carbon black masterbatch and 0.5–1.0 wt% of a processing aid masterbatch, yielding 2.0–2.5 wt% final carbon black in the pipe wall. The melt is extruded through a die head into a moving corrugator with vacuum forming blocks at -0.02 to -0.05 MPa; melt temperature is held at 200–225°C, and corrugator line speed is 0.5–3.0 m/min for diameters from DN 100 to DN 800. A 1.5% deviation in corrugator speed changes corrugation pitch by 4–6 mm on DN 300 pipe, which is detected by in-line laser profilometry and rejected before perforation. After forming, drainage slots are cut or punched into the outer crown, and the finished pipe is tested for ring stiffness and joint tightness. Terminal product types include stormwater culverts, agricultural field drainage, cable ducting, and landfill leachate collection pipes. The applicable compliance framework is ASTM F2306-19, AASHTO M294-20, and EN 13476-3:2018 for structured-wall polyolefin pipes; soil-tight and water-tight joint performance is verified by the specific test protocols in those standards. A field bottleneck occurs when the corrugator vacuum is reduced by build-up of carbon black fines on the forming blocks; the condition produces thin spots in the pipe wall and requires a cleaning interval of 8 h on long runs. In addition, the grade should not be processed with screw speeds that force melt temperature above 225°C, because low-molecular-weight species generated by oxidative chain scission lower the local melt strength and cause corrugation collapse before the water spray cooling zone.
Industrial monofilament extrusion from HD5503S is constrained by the relationship between quench temperature, draw ratio, and final filament tenacity. A representative formulation contains 97.0–99.0 wt% HD5503S, 0.5–2.0 wt% UV-stabilised colour masterbatch, and 0.2–0.5 wt% of an antioxidant-processing aid masterbatch; polypropylene is excluded because its lower melt viscosity disrupts the HDPE crystalline network and causes fibrillation during drawing. The resin is fed to a single-screw extruder with L/D 24:1–30:1 and a spinneret hole diameter of 0.8–1.2 mm; melt temperature is 190–220°C. Extruded filaments pass through a water quench bath at 35–50°C, then enter a two-stage hot drawing system at 90–115°C with total draw ratio of 7:1–10:1; a relaxation zone of 2–4% on heated godets stabilises filament diameter. When the draw ratio exceeds 9:1, die-lines and surface shark-skin become detectable unless the quench bath temperature is raised to the upper end of the range; drawing above 115°C reduces orientation and lowers tenacity below 0.25 N/tex in the final filament. Published data for HD5503S specifically in monofilament drawing is limited; the cited draw ratios and bath temperatures are operating windows for high-molecular-weight HDPE of similar melt flow rate and density rather than grade-specific design values. Terminal products include agricultural netting, industrial rope and twine, fishery cage netting, and brattice cloth for mine ventilation. The applicable product standard is ASTM D3218-07 for polyolefin monofilaments, supplemented by standard lot testing of diameter variation and tensile strength. A known processing failure occurs when the quench bath temperature drops below 30°C: the skin freezes too quickly, preventing uniform drawing and producing filament diameter variation above 12%, which is outside the acceptable range for netting conversion.
Competitive Yanchang China Coal Yulin (Shaanxi) HDPE HD5503S prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Yanchang China Coal Yulin (Shaanxi) HDPE HD5503S is a high-density ethylene copolymer produced at the Yulin coal-to-olefins facility in Shaanxi Province. The grade is intended for extrusion blow molding of rigid containers from 100 mL to 5 L, including household chemical bottles, personal-care containers, and small food-contact packaging. Product-specific technical literature lists the design density at 0.955 g/cm³ and the melt mass-flow rate at 0.35 g/10 min under 2.16 kg at 190 °C. These values place HD5503S in the high-stiffness segment of blow-molding HDPE, separated from medium-density polyethylene by a larger solid-state modulus and from high-flow injection-molding HDPE by higher melt strength and longer parison hang time. The material is not a general-purpose grade; its process window is tuned for a narrow balance of die swell, parison stability, and container crush resistance. It is used primarily in packaging applications requiring resistance to environmental stress cracking in aqueous surfactant and mild chemical environments. The grade is not intended for blown film, sheet, or injection molding.
| Property | Test method | Typical range |
| Melt mass-flow rate | ISO 1133-1:2022, 190 °C/2.16 kg | 0.30–0.35 g/10 min |
| Density | ISO 1183-1:2019 | 0.954–0.956 g/cm³ |
| Tensile yield stress | ISO 527-2:2012, type 1A, 50 mm/min | 26–28 MPa |
| Elongation at break | ISO 527-2:2012 | >600% |
| Flexural modulus | ISO 178:2019 | 1,000–1,200 MPa |
| ESCR F50 | ASTM D1693-15 condition B, 10% Igepal | >100 h |
| Vicat softening point | ISO 306:2022 A50 | 124–128 °C |
Values in the table are typical design targets from producer technical literature for the 5503S designation and should be confirmed against the producer’s certificate of analysis for each lot. Lot-to-lot variation in density is usually held within ±0.001 g/cm³, while melt flow rate variation is typically controlled within ±0.03 g/10 min in continuous slurry polymerization.
Output is governed by melt temperature and screw torque rather than by feed capacity. On shuttle blow molders equipped with 60 mm to 90 mm grooved-barrel extruders, the practical melt-temperature ceiling is 215–220 °C; operation above 220 °C accelerates thermo-oxidative chain scission, reducing melt viscosity and increasing parison sag. The low melt flow rate of 0.30–0.35 g/10 min produces higher melt pressure and gearbox load than 0.7 g/10 min blow-molding HDPE at the same screw speed. For this density class, onset of surface melt fracture in straight dies is reported at apparent wall shear stresses of 0.15–0.25 MPa; die gaps below 1.0 mm at high output can produce shark-skin surface defects on bottle surfaces. Published output-rate curves for this specific grade are limited, so maximum continuous screw speed should be established on the target machine with melt temperature override as the controlling limit.
Die swell and parison length uniformity are controlled by the temperature gradient from the extruder to the die bushing. A representative barrel profile is 170/185/195/200 °C from feed to metering, with head and die zones at 190–205 °C. Blow air pressure is set between 0.6 MPa and 0.8 MPa, while mold temperatures are held at 10–25 °C for rapid solidification. At 200 °C melt temperature, parison hang times up to 8 s are generally workable; longer hang times are accommodated by reducing melt temperature within the 195–200 °C band and by increasing the die gap. The grade’s low MFR supports parison integrity better than 0.7 g/10 min blow-molding HDPE, but it demands more extruder torque and may lower output in small extruders with limited gearbox service factor. Regrind levels above 30% can reduce ESCR and melt strength, and must be validated for the final container geometry and fill environment.
The 0.955 g/cm³ density of HD5503S produces a flexural modulus of 1,000–1,200 MPa when tested by ISO 178:2019, which is substantially higher than MDPE blow-molding grades in the 0.934–0.940 g/cm³ density range. This modulus increase supports greater column crush resistance at equal wall thickness. However, top-load capacity in a molded container is not a direct function of resin modulus alone; wall-thickness distribution, pinch-off weld geometry, and handle design control the observed crush force. Converters characterize empty-container top-load strength by ASTM D2659-16 or equivalent compression methods. Published data for a specific bottle configuration using HD5503S is limited; comparative molded-part trials are required when replacing a lower-density grade because the higher stiffness can be accompanied by reduced stress-crack resistance and lower low-temperature ductility.
| Material class | Density (g/cm³) | MFR (g/10 min at 190 °C/2.16 kg) | Flexural modulus (MPa) | Typical processing boundary |
| HD5503S | 0.954–0.956 | 0.30–0.35 | 1,000–1,200 | Extrusion blow molding, small rigid containers |
| MDPE blow-molding grade | 0.934–0.940 | 0.5–0.8 | 500–700 | Large-part blow molding requiring high ESCR |
| High-flow injection HDPE | 0.955–0.960 | 18–25 | 1,200–1,500 | Thin-wall injection molding, caps, closures |
Compared with a typical MDPE blow-molding resin of 0.938 g/cm³ density and 0.7 g/10 min MFR, HD5503S offers higher stiffness and better parison hang strength, but generally lower ESCR and lower low-temperature impact resistance. Compared with a high-flow injection-molding HDPE of 20 g/10 min MFR, HD5503S cannot fill thin-wall multi-cavity molds with long flow paths because its spiral flow length is substantially shorter; the injection-molding grade conversely lacks sufficient melt strength for blow molding. The comparison table summarizes representative class ranges, not exact lot data. Selection among these materials is governed by the processing route and the required combination of container crush resistance and stress-crack resistance.
In extrusion blow molding, the pinch-off weld is the weakest structural zone in the base of a bottle. For HD5503S at 200 °C melt temperature and 0.6–0.8 MPa blow pressure, pinch-off weld strength depends on mold clamping force and pinch insert profile; insufficient clamp force allows molten polymer to escape the parting line, creating a thin or rough flash line. On machines with hydraulic clamp force below 150 kN for bottles with 1.0 mm wall thickness, pinch-off flash may be incompletely compressed, reducing drop-impact resistance at -20 °C when tested by ASTM D2463-15. Published data for a specific HD5503S pinch-off configuration is limited; burst and drop tests must be performed on production closures.
Water vapor barrier of HDPE is governed by density and thickness. At 0.955 g/cm³, the grade transmits less water vapor than lower-density HDPE, but it remains a hydrocarbon polymer and is not a barrier to oxygen, carbon dioxide, or organic solvents. For oxygen-sensitive contents, a coextruded structure with EVOH or polyamide is required. The water vapor transmission rate through a 1 mm HDPE sheet at 38 °C and 90% RH is commonly reported in the range of 0.2–0.5 g·mm/(m²·day) when normalized to thickness; actual container WVTR depends on sidewall thickness and orientation.
HD5503S is typically selected for containers in contact with aqueous surfactants, mild acids, and dilute alkalis. Environmental stress-cracking resistance, measured by ASTM D1693-15 condition B with 10% Igepal CO-630 at 50 °C, is typically above 100 h for this density class. The grade is not a substitute for high-molecular-weight HDPE or MDPE in aggressive stress-cracking environments such as concentrated detergents, organic solvents, or strong oxidizing acids. Chemical compatibility must be tested in the final container geometry with the actual fill composition, because molded-in stress and wall thickness interact with the stress-cracking environment in ways that resin data alone cannot predict. The material is not inherently transparent; containers are typically pigmented or fitted with surface labels. Where optical clarity is required, a clarified polypropylene random copolymer or PET is commonly used, but those materials have different drop-impact, stress-cracking, and sealing behavior.
Food-contact compliance is evaluated on the finished article under FDA 21 CFR 177.1520(c) 3.1a and, for the EU market, under Commission Regulation (EU) No 10/2011 with the overall migration limit of 10 mg/dm² or 60 mg/kg for food simulants. For China, GB 4806.6 applies to food-contact polyethylene and sets overall migration limits for the intended contact conditions. The resin is supplied as natural or formulated with specific additive packages; converters must verify organoleptic and extraction performance with the intended food simulant. The grade is not formulated for prolonged outdoor exposure; if UV stabilization is required, a UV-stabilized variant or a compounded masterbatch must be used. Drying is not usually required for sealed hopper storage, but material exposed to relative humidity above 60% or stored in open silos should be dried at 80 °C for 2 h before processing to prevent surface defects from water vapor.