Yanchang China Coal Yulin Shaanxi Hdpe G50 120

Yanchang China Coal Yulin (Shaanxi) HDPE G50-120

    • Product Name: Yanchang China Coal Yulin (Shaanxi) HDPE G50-120
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 100895
    Product Name Yanchang China Coal Yulin (Shaanxi) HDPE G50-120
    Manufacturer Yanchang China Coal Yulin Energy and Chemical Co., Ltd.
    Material High-Density Polyethylene (HDPE)
    Grade G50-120
    Form Pellets
    Density 0.950-0.952 g/cm³
    Melt Flow Rate 10-14 g/10 min (190°C/2.16 kg)
    Melting Point 130-135°C
    Vicat Softening Temperature ≥120°C
    Tensile Yield Strength ≥25 MPa
    Elongation At Break ≥500%
    Flexural Modulus ≥1000 MPa
    Notched Impact Strength ≥50 J/m (23°C)
    Hardness ≥60 Shore D
    Thermal Deformation Temperature ≥70°C
    Water Absorption <0.01%
    Color Natural

    As an accredited Yanchang China Coal Yulin (Shaanxi) HDPE G50-120 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Yanchang China Coal Yulin (Shaanxi) HDPE G50-120 is packed in 25 kg PP woven bags, 1000 kg per pallet.
    Container Loading (20′ FCL) Container Loading (20′ FCL): Yanchang China Coal Yulin (Shaanxi) HDPE G50-120, 25kg bags, total 25MT.
    Shipping Yanchang China Coal Yulin (Shaanxi) HDPE G50-120 is shipped as non-hazardous thermoplastic pellets in 25 kg bags or 1,000 kg jumbo bags, palletized and stretch-wrapped. Transport in clean, dry containers/trucks; keep away from moisture, heat, sunlight, and contamination. Standard export packing; no special dangerous goods documentation required.
    Storage Store Yanchang China Coal Yulin (Shaanxi) HDPE G50-120 in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and ignition sources. Keep original bags closed, palletized, and off the floor. Protect from moisture, dust, oils, and contaminants. Avoid prolonged high temperatures and heavy stacking. Use appropriate PPE and follow local regulations.
    Shelf Life Shelf life is 24 months from production date when stored cool, dry, ventilated, sealed, and protected from sunlight, moisture, and contamination.
    Application of Yanchang China Coal Yulin (Shaanxi) HDPE G50-120

    Yanchang China Coal Yulin (Shaanxi) HDPE G50-120 is assigned to high-flow injection-molding applications in which a nominal density of 0.950 g/cm³ (ISO 1183-1:2019) and a melt mass-flow rate of 12 g/10 min at 190 °C/2.16 kg (ISO 1133-1:2022) permit filling of multi-rib geometries at practical clamping forces. The scenarios that follow exclude film, blow molding, pipe extrusion, and rotomolding because the grade is not formulated for those processes. All additive mass fractions are expressed as a percentage of the total compound. Resin stored at relative humidity above 60% RH is pre-dried at 80 °C for 2 h before processing; surface moisture that remains on un-dried granulate produces splay and gate blush on gloss surfaces.

    Stacking load retention in returnable industrial crates

    Returnable industrial crates and logistics totes represent the largest injection-molding segment for HDPE G50-120. The compounding ratio is set at 96.0–98.5 wt% HDPE G50-120, 1.0–3.0 wt% pigment or carbon black masterbatch, 0.10–0.40 wt% hindered amine light stabilizer, and 0.05–0.20 wt% primary antioxidant. Compliance testing for loaded crates references ASTM D642-20 for compressive resistance, ASTM D638-14 for tensile yield stress, and ASTM D790-17 for flexural modulus; where crates are used as unit-load bases under racking conditions, ISO 8611-1:2021 is applied to the assembled load. On production-scale 800 t toggle-clamp injection machines with cold sprue bushings, melt temperature is held at 210–250 °C and mold temperature is maintained at 15–60 °C. The main process conflict is that sidewall thicknesses of 6–10 mm generate sink marks at boss-rib intersections if holding-pressure transfer occurs after gate freeze. Gate freeze time in unfilled HDPE at 3.0 mm wall is approximately 8–12 s; holding pressure is therefore sustained at 60–110 MPa until the gate freezes. Finished product types include 600×400 mm and 800×600 mm returnable distribution crates, agricultural picking totes, bread trays, and collapsible side-wall logistics boxes molded with vertical ribs for stacking heights of up to 5 units.

    In thin-wall dairy and spreads packaging, HDPE G50-120 is processed on high-speed accumulator-assisted injection machines with 24:1 L/D barrier screws and stack molds running 4+4 cavities to fill wall sections of 0.7–1.3 mm without exceeding practical injection pressure. The compound is set at 98.0–99.5 wt% virgin HDPE G50-120, 0.05–0.20 wt% nucleating agent to raise crystallization onset temperature and reduce demolding distortion, and 0.5–1.5 wt% slip/antiblock masterbatch. Melt temperature is 220–260 °C, mold temperature is 8–25 °C, injection velocity is 180–320 mm/s, and total cycle time for 250–1,000 g tubs is 4.5–8.0 s. Thermal balance between parting lines is maintained with coolant flow of 15–25 L/min per cavity circuit to prevent plate deflection and uneven gate freeze. Compliance for this sector requires FDA 21 CFR 177.1520 for olefin polymer food-contact authorization, EU 10/2011 with overall migration limit of 10 mg/dm², and GB 9685-2016 for additives used in food-contact materials; heavy-metal pigment dispersions are excluded because extraction limits for antimony, arsenic, and cadmium are specified under EU 10/2011. Terminal products include 150–500 ml dairy cups, 250–1,000 g margarine and spreads tubs, and deli containers closed with snap-on HDPE lids.

    Standard/RegulationTest or PropertyNumerical Limit or Designation
    FDA 21 CFR 177.1520Olefin polymer food-contact authorizationResin manufacturer food-contact statement required
    EU 10/2011Overall migration10 mg/dm²
    GB 9685-2016Additive positive listOnly listed additives permitted

    What limits high-cavitation cap molding when torque retention is specified?

    Closure molding with HDPE G50-120 in 32, 48, or 64-cavity valve-gated hot-runner tools is constrained by the trade-off between melt flow and environmental stress crack resistance. The base compound ratio is 95.0–98.5 wt% HDPE G50-120, 1.0–3.0 wt% polyolefin elastomer or LLDPE to raise ESCR, 0.02–0.10 wt% slip additive, and 1.0–2.5 wt% color masterbatch. Processing is carried out at melt temperature 230–260 °C, injection velocity 120–250 mm/s, and mold temperature 10–30 °C; total cycle time is 6–12 s. Nozzle melt temperature is maintained 5–15 °C above the set front-zone temperature to offset shear heating at the valve gate. The gate-freeze time at a 0.8–1.2 mm annular gate land is shorter than in thin-wall packaging, and premature holding-pressure release produces dimensional ovality in 28 mm and 38 mm tamper-evident closures. Compliance references ISO 8317:2015 for child-resistant packaging, ASTM D3475-20 for the classification of child-resistant package types, and FDA 21 CFR 177.1520 for food-contact caps; for pharmaceutical closures, USP 661.1 plastic packaging materials is applied. Torque retention is not defined by a single published value for this grade; strip torque, removal torque, and leak pressure are closure-specific and must be established on the actual liner and bottle finish combination. Finished product types include tamper-evident beverage closures in 28 mm and 38 mm, child-resistant pharmaceutical caps, push-pull sports closures, and household chemical closures with lined or linerless seals.

    Open-top pails molded from HDPE G50-120 are qualified for dangerous-goods packaging only after passing a sequence of drop, leakproofness, and stacking tests under UN Model Regulations and the IMDG Code for packing group II or III, depending on fill mass and specific gravity. The formulation for this sector uses 94.0–97.0 wt% HDPE G50-120, 2.0–5.0 wt% LLDPE or metallocene polyethylene as impact modifier, 0.1–0.3 wt% antioxidant, and 1.0–3.0 wt% pigment masterbatch. Processing occurs in 500–1,000 t injection machines with hydraulic core-pull systems and in-mold labeling capability; melt temperature is 220–250 °C, mold temperature is 10–45 °C, and cycle time is 30–60 s for 15–25 L pails. In-mold labeling with polypropylene or paper labels introduces gas entrapment at the pail base if vent depth is below 0.01 mm; vacuum-venting in the core is used when label coverage exceeds 80% of the sidewall. The main process conflict is that impact modification for low-temperature drop performance at -18 °C reduces flexural modulus; handle anchorage bosses therefore require locally thicker ribs, but excessive rib thickness at the handle base creates sink marks on the pail exterior. Drop testing follows ASTM D5276-19, and stacking tests are carried out to ASTM D642-20 on filled, closed pails. Terminal product types include 5 L, 10 L, 15 L, 20 L, and 25 L open-top pails, UN-certified round and rectangular pails for paints, lubricants, food ingredients, and water-based industrial chemicals, with injection-molded lids incorporating tear-strip tamper evidence.

    When phthalate-free toy components require low-temperature impact compliance

    Injection-molded toy components produced from HDPE G50-120 require a formulation that avoids phthalate plasticizers entirely, because REACH Annex XVII entries 51 and 52 restrict certain phthalates in toys and childcare articles. The compounding ratio is 96.0–99.0 wt% HDPE G50-120, 0.05–0.20 wt% non-phthalate nucleating agent, 0.5–2.0 wt% color masterbatch, and 0.05–0.15 wt% antioxidant. Migration-of-elements testing is carried out to EN 71-3:2019+A1:2021 and ASTM F963-23; category-specific limits for lead, cadmium, and barium are applied according to the final toy material classification. Processing uses melt temperature 200–240 °C and mold temperature 10–30 °C. The low melt temperature is selected to limit color-degradation byproducts that can affect the migration profile and surface gloss. Color masterbatch carriers are specified as PE-based rather than EVA-based because an LDPE carrier at 2 wt% can lower heat deflection temperature by approximately 3–5 °C. The main technical limitation is that HDPE G50-120 has lower low-temperature impact than grades with higher molecular weight; components with snap-fit tabs or thin living hinges are therefore limited to radii above 0.8 mm at the hinge root when evaluated at -20 °C under ISO 180:2019. Terminal product types include building blocks, stackable toy storage boxes, outdoor play components, and toy vehicle bodies in which high-gloss surfaces and migration-limited element release are simultaneously specified.

    Household storage bin ribbing and wall-stiffness optimization

    Household storage articles molded from HDPE G50-120 are designed around snap-on lid retention and stackability under residential load. The compounding ratio is 97.0–99.0 wt% HDPE G50-120, 1.0–2.0 wt% antistatic masterbatch, and 1.0–2.0 wt% color masterbatch; no external lubricant is added because lid engagement force is controlled by part geometry rather than surface slip. Melt temperature is 210–250 °C, mold temperature is 20–50 °C, and injection speed is reduced to 40–120 mm/s on 250–500 t toggle machines to minimize flow marks on large visible sidewalls. Excessively low injection speed at the lower limit of 40 mm/s causes short shots in thin-wall ribs; velocity profiling is therefore ramped after 70% fill to maintain flow-front continuity. Compliance relies on REACH Annex XVII and, where applicable, California Proposition 65 for chemical exposure from storage of consumer goods; mechanical verification uses ASTM D638-14 for tensile yield, ASTM D790-17 for flexural modulus, and ASTM D256-10 for notched Izod impact. The main processing fault is warpage along the long axis of molded sidewalls; this is corrected by rib pitch below 50 mm and wall-to-rib thickness ratios above 1:0.6 to avoid sink and differential shrinkage. Terminal product types include modular stackable storage bins with lidded and open designs, under-bed storage containers, garment organizers, and garage storage modules in volumes from 10 L to 145 L.

    Free Quote

    Competitive Yanchang China Coal Yulin (Shaanxi) HDPE G50-120 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Yanchang China Coal Yulin (Shaanxi) HDPE G50-120 is a high-flow high-density polyethylene injection-molding resin produced at the coal-to-olefins complex in Yulin, Shaanxi Province. The grade designation is read as a nominal density of 0.950 g/cm³ and a nominal melt flow rate of 12.0 g/10 min at 190°C/2.16 kg under ISO 1133-1:2022. The resin is supplied as natural white granules with a narrow molecular weight distribution designed for rapid cavity filling in thin-wall injection molding, caps, closures, housewares, crates, and general-purpose injection articles. Published data for this specific configuration is limited; the product is not designed for load-bearing pipe applications, and it should not be assigned a PE100 hydrostatic classification under ISO 9080:2012 without separate formulation-specific validation.

    Compared with medium-flow HDPE injection grades of similar density, G50-120 shifts the processing-property balance toward higher cavity-fill capacity at lower injection pressure. The higher melt flow index reduces apparent viscosity at commercial shear rates, but it also lowers notched impact performance relative to lower-melt-flow HDPE grades. That trade-off must be specified through the application-specific impact test rather than inferred from the grade designation alone. For food-contact and pharmaceutical packaging, the natural unpigmented resin must be certified against the relevant national food-contact regulation before production because color concentrates and processing aids can alter compliance status.

    The product belongs to a portfolio derived from methanol-to-olefins conversion, and the polymerisation reactor system controls the comonomer distribution such that the grade remains within a density band suitable for rigid articles. Batch-to-batch variation in melt flow rate is typically controlled within the manufacturer’s release window, but converters running thin-wall containers should request the actual certificate of analysis for each lot because even 0.5 g/10 min MFR drift changes fill pressure and part mass.

    What Limits Cycle-Time Reduction When G50-120 Replaces Medium-Flow HDPE?

    Replacement of a 5.0 g/10 min HDPE grade with G50-120 in multi-cavity injection tooling typically permits a reduction in injection pressure and hold time. On a 2200 kN electric toggle press equipped with a 40 mm general-purpose screw of 23:1 L/D, melt temperature can be set from 180°C to 220°C. At the lower boundary, the cavity may short-fill in narrow ribs and valve-gated drops; at the upper boundary, flash can appear on parting lines and the cooling load increases. The practical melt setpoint therefore falls between 190°C and 210°C for most thin-wall tools with wall stock below 1.5 mm.

    Spiral flow length at 190°C and 80 MPa injection pressure is substantially longer than that of medium-flow HDPE at the same melt temperature. The high MFR of 12.0 g/10 min reduces fill pressure drop across long flow paths, allowing thinner nominal wall sections without increasing clamp force. However, melt-flow length is not the only cycle determinant. The cooling time remains proportional to the square of wall thickness, so reducing wall thickness from 1.8 mm to 1.2 mm can cut theoretical cooling time by more than half, while G50-120 supplies the lower viscosity needed to achieve that fill.

    The shear viscosity at 1000 s⁻¹ and 200°C is lower than that of a 5.0 g/10 min grade by roughly 20–30% when measured using ISO 11443:2021 capillary rheometry. This difference is most visible in thin-wall parts where flow-length-to-wall-thickness ratios exceed 150:1. In hot-runner closure tooling with 96 cavities, melt-flange temperature variation of ±5 K produced cavity mass variation exceeding 0.02 g; balance was restored by raising valve-gate dwell to 0.35 s. That production-specific observation illustrates that lower viscosity does not eliminate the need for thermal uniformity in the hot half.

    The process window is bounded by two competing failure mechanisms. At melt temperature below 180°C, the frozen skin closes off flow in hinge areas and bosses. At melt temperature above 220°C or residence time longer than 10 min, oxidative degradation can increase the melt flow index and cause yellowing. A melt-temperature probe inside the nozzle, rather than a barrel zone setting, should be used to verify the actual melt temperature because shear heating can raise local temperature by 8–15 K at high screw recovery speeds.

    Mechanical specification for G50-120 is controlled by the manufacturer’s certificate of analysis, and the comparative engineering values below are typical for the resin class rather than batch-specific limits. In injection-molded parts subjected to compressive stacking, the flexural modulus determines sidewall deflection under load; for snap-fit features, tensile yield stress controls insertion and removal force. The property set can be positioned relative to adjacent melt-flow HDPE grades using the following data.

    Comparative nominal properties for Yanchang China Coal Yulin HDPE G50-120 and adjacent melt-flow HDPE injection grades. The manufacturer’s batch certificate is the controlling specification.
    Property G50-120 nominal Medium-flow HDPE injection grade High-flow HDPE injection grade Test method
    Melt flow rate, 190°C/2.16 kg 12.0 g/10 min 5.0 g/10 min 20.0 g/10 min ISO 1133-1:2022
    Density 0.950 g/cm³ 0.954 g/cm³ 0.952 g/cm³ ISO 1183-1:2019
    Tensile yield stress 26 MPa 28 MPa 25 MPa ISO 527-2:2012
    Flexural modulus 1150 MPa 1250 MPa 1100 MPa ISO 178:2019
    Charpy notched impact strength, 23°C 3.5 kJ/m² 6.0 kJ/m² 2.5 kJ/m² ISO 179-1:2023
    Vicat softening temperature, A50 126°C 127°C 124°C ISO 306:2022
    Heat deflection temperature, 0.45 MPa 75°C 78°C 72°C ISO 75-2:2013
    Molding shrinkage, parallel flow 1.8–2.2% 1.6–2.0% 1.8–2.4% ISO 294-4:2018

    The lower flexural modulus of G50-120 relative to medium-flow HDPE is a direct consequence of its lower density and higher melt flow; it is not a processing defect. When stacking strength governs a crate or box design, sidewall deflection should be calculated with the flexural modulus from the batch certificate and corrected for molding orientation. Weld lines in high-flow HDPE are typically weaker than in medium-flow HDPE because the faster melt front cools and freezes before sufficient intermolecular diffusion occurs at the meeting plane.

    Where Thin-Wall Impact and Stacking Strength Must Be Verified

    For closures and thin-wall dairy containers, the grade is often selected for spiral flow and cycle time, but impact performance must be verified at the actual wall thickness. Instrumented puncture testing on 1.0 mm plaques according to ISO 6603-2:2016 at 23°C provides a better prediction of container cracking than notched Charpy data. Published data for this specific configuration is limited; converters should obtain internal plaque puncture data for the individual mold and cooling rate. In general, the transition from a 5.0 g/10 min HDPE grade to G50-120 can reduce impact force at equivalent wall thickness by 10–20%, so thinning the wall solely on the basis of MFR is not justified without impact validation.

    Stacking strength of boxes and crates is a structural property governed by sidewall buckling, not melt flow. G50-120, with nominal flexural modulus near 1150 MPa, can be used for crates if wall thickness and rib geometry are retained. However, compared with a medium-flow HDPE grade with flexural modulus near 1250 MPa, the lower modulus produces additional deflection at the same load, requiring either a 6–8% thicker wall or a different rib pattern to achieve the same top-load resistance. Compression capacity of stackable containers should be measured under ISO 12048:1994 with a closed-loop universal testing machine and a 10 mm/min platen speed, because hand-stacking trials do not separate short-term buckling from creep.

    Environmental stress-cracking resistance for G50-120 is lower than that of medium-flow HDPE. Applications involving detergents, surfactants, or lye at elevated temperatures require batch-specific ASTM D1693 condition B testing; published data for the specific grade in those media is limited. For closure applications, torque retention and liner adhesion should be evaluated on the actual cap geometry after contact with the filled product. The high-flow HDPE grade should not be used in pipe or fitting applications requiring hydrostatic strength under ISO 9080:2012, because its molecular weight and tie-molecule concentration are optimized for injection molding rather than long-term creep rupture resistance.

    Hopper drying is not required for dry resin, but surface condensation from outdoor silo storage in northern Shaanxi is more relevant than bulk moisture absorption. If pellet surface temperature is below ambient dew point, moisture can produce splay and silver streaks. Pre-drying at 70°C for 1–2 h in a desiccant hopper dryer is recommended when the resin has been stored in unheated silos during winter or at relative humidity above 60%.

    Melt temperature should be controlled at 190–210°C for most molding operations. A barrel profile of 180–200°C from rear to front, nozzle at 200°C, and screw back pressure of 0.5–1.5 MPa can maintain a stable melt cushion. Injection speed should be set to fill thin sections within 0.1–0.3 s, but high shear rates can generate melt burn; capillary shear rates above 1000 s⁻¹ should be reviewed with ISO 11443:2021 rheometry before permanent tool changes. Mold temperature of 20–40°C is typical. Mold temperature below 15°C freezes the skin too quickly and intensifies flow lines, weld-line weakening, and differential shrinkage. Mold temperature above 60°C can improve impact and weld-line strength but increases cooling time and may require post-mold shrinkage adjustment.

    The resin is incompatible with polypropylene, PET, or PVC residues; segregated material handling is required. Purging with low-MFR LDPE or a commercial HDPE purge grade after color or material changes is recommended. If an emergency stop leaves melt in the barrel at 220°C for more than 10 min, the holdup should be purged before restarting to avoid degraded gels in the next parts.

    Food-Contact and Regulatory Status Under Standard-Based Verification

    The natural unpigmented G50-120 grade, as an olefin polymer, can be evaluated for food-contact use under standard food-contact regimes applicable to high-density polyethylene. Compliance is not a single universal declaration; it depends on the final additive package, color masterbatch, processing residues, and intended temperature-time conditions. The following checklist is used in production release documentation when the resin is supplied for food packaging.

    Regulatory verification framework for natural G50-120 in food-contact and general articles. Final compliance must be confirmed by the converter for the exact formulation and use condition.
    Regulation/standard Scope Test or clause Typical release criterion
    EU REACH 1907/2006/EU SVHC reporting Article 33 No SVHC above 0.1% w/w in natural resin
    RoHS 2011/65/EU Heavy metals and brominated flame retardants Directive Annex II Pb, Cd, Hg, Cr(VI) below limit values by XRF screening
    FDA 21 CFR 177.1520 Olefin polymers for food contact Subsection (c) End-use food contact under specified conditions, no unauthorized colorants
    China GB 4806.7-2016 Food-contact plastic materials Overall migration <10 mg/dm² for general food simulants under intended conditions

    The regulatory table does not replace batch-specific compliance certificates. For food-contact applications, the converter must perform overall migration testing on the finished article after all colorants, additives, and processing aids have been incorporated; residual stress, heat history, and wall thickness can modify migration behavior. G50-120 should not be combined with recycled post-consumer HDPE in food-contact applications unless the recyclate is separately approved under the applicable jurisdiction.

    Top