| HS Code | 310367 |
| Density | 0.870 g/cm³ |
| Melt Index 190 C 2 16 Kg | 1.5 g/10 min |
| Shore A Hardness | 75 |
| Shore D Hardness | 20 |
| Tensile Strength At Break | 8.0 MPa |
| Tensile Elongation At Break | 800% |
| Flexural Modulus | 15 MPa |
| Vicat Softening Point | 50°C |
| Melting Point | 60°C |
| Glass Transition Temperature | -55°C |
| Crystallinity | 15% |
| Tear Strength | 40 kN/m |
| Haze | 2% |
| Gloss 45 | 80% |
As an accredited Westlake Mxsten® CV77515-F Plastomer factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Westlake Mxsten® CV77515-F Plastomer is packaged in 25 kg polyethylene bags, 40 bags per pallet, or 1,000 kg bulk bags. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with Westlake Mxsten® CV77515-F Plastomer in palletized bags, securely stowed and braced for ocean transport. |
| Shipping | Westlake Mxsten® CV77515-F Plastomer is typically shipped as non-hazardous solid pellets. It is packaged in 25-kg bags, octabins, or bulk containers, and transported in clean, dry trucks or containers at ambient temperature. Protect from moisture, contamination, and direct sunlight. Consult the SDS for exact shipping classification. Keep containers sealed. |
| Storage | Store Westlake Mxsten® CV77515-F Plastomer in a cool, dry, well-ventilated area, away from direct sunlight, heat, ignition sources, and incompatible materials. Keep containers closed to prevent moisture, dust, and contamination. Avoid prolonged high temperatures to minimize caking or degradation. Protect packaging from damage, do not overstack, and follow first-in, first-out rotation plus manufacturer’s SDS instructions. |
| Shelf Life | Westlake Mxsten® CV77515-F Plastomer has a recommended shelf life of 24 months when stored unopened under cool, dry conditions. |
In three-layer blown-film coextrusion lines operating above 80 m/min, Westlake Mxsten® CV77515-F Plastomer is introduced into the sealant skin as a partial replacement for Ziegler-Natta LLDPE, typically at 10 wt% to 30 wt%, or is run as the dominant sealant web with 5 wt% to 15 wt% LDPE added to stabilize bubble geometry. The grade belongs to the ethylene-1-octene metallocene plastomer class; supplier literature lists a nominal density of 0.875 g/cm³ under ASTM D792 and a melt mass-flow rate of 1.5 dg/min at 190°C/2.16 kg under ISO 1133-1:2022. The processing window on a 45 mm barrier screw with 30:1 L/D and a Maddock mixing section uses barrel temperatures from 160°C to 220°C, die temperatures between 185°C and 215°C, a die gap of 1.8 mm to 2.5 mm, and a blow-up ratio from 2.0:1 to 3.0:1. Frost-line height is normally held at 4 to 8 die diameters because excessively high frost lines in low-density sealant webs produce backside blocking and reel-hardness variation. Food-contact sealing webs must comply with FDA 21 CFR 177.1520(c) for olefin polymers and EU 10/2011, with overall migration limited to 10 mg/dm² under the intended time-temperature conditions; industrial non-food structures are verified under REACH Regulation (EC) No 1907/2006 and RoHS Directive 2011/65/EU. Heat-seal strength is characterized by ASTM F88/F88M and heat-seal initiation curves by ASTM F2029, with dwell time of 0.5 s and jaw pressure of 0.275 MPa used as starting conditions; exact seal initiation temperatures for CV77515-F are obtained from the current supplier seal curve because the measured value shifts with coextruded substrate gauge, tie-layer thickness, and jaw configuration. Major failure modes observed on production lines include melt fracture at the die lip when the skin layer exceeds 30 wt% plastomer, die-lip buildup on the outer die during prolonged runs above 220°C, and blocking on the collapsing frame when the film is wound with excessive residual heat. End-product types include vertical form-fill-seal pouches for frozen and dry food, lidding films for polypropylene cups, and high-speed horizontal flowrap overwrap where low seal initiation and broad hot-tack behaviour are required.
| Application | Standard or regulation | Clause or test method | Measured parameter |
|---|---|---|---|
| Food-contact flexible packaging | FDA 21 CFR 177.1520 | Paragraph (c), olefin polymers | Extractables and migration limits |
| Food-contact flexible packaging | EU 10/2011 | Annex I, overall migration | 10 mg/dm² overall migration |
| Automotive interior PP compounds | VDA 278 | Thermal desorption analysis | VOC and fogging residue |
| PP impact characterization | ISO 179-1 / ASTM D256 | Notched impact | kJ/m² or J/m |
| Hot-melt adhesives for packaging | FDA 21 CFR 175.105 | Adhesives in food contact | Regulatory composition and migration |
| Crosslinked polyolefin foam | ASTM D2765 | Solvent extraction | Gel fraction |
| Low-voltage cable compounds | IEC 60811-501 | Tensile and elongation | Mechanical integrity after ageing |
| Environmental compliance | RoHS Directive 2011/65/EU | Annex II | Restricted substance thresholds |
Compounding CV77515-F into unfilled PP homopolymer at 10 wt% to 20 wt% is the standard range for interior automotive and appearance parts where low-temperature notched impact is prioritized over stiffness. In talc-filled PP formulations containing 15 wt% to 25 wt% talc, the plastomer is more commonly added at 10 wt% to 15 wt% because higher loadings reduce flexural modulus without a proportional gain in impact. The compounding line uses a co-rotating twin-screw extruder with 40:1 L/D and segmented screws; barrel temperatures are set from 180°C to 220°C, screw speed from 400 rpm to 600 rpm, and pelletizing is conducted through an underwater die at 180°C. A high-shear mixing zone followed by a distributive kneading block is used to reduce plastomer domain size; SEM examination of n-heptane-etched microtomed sections should show dispersed domains below 2 µm for consistent ductile behaviour. Injection moulding of test plaques and components is performed according to ISO 294-1 at melt temperatures of 200°C to 230°C, mould temperatures of 20°C to 40°C, and clamp force settings determined by gate size and flow length. Notched impact is measured by ISO 179-1 or ASTM D256; for filled compounds, the ductile-to-brittle transition is mapped by testing at -30°C, -20°C, and 0°C. Published data for this specific configuration is limited, but compounding trials generally show that 10 wt% plastomer in a 15 wt% talc-filled PP shifts the ductile-to-brittle transition below -20°C only when the screw configuration avoids coalescence of plastomer domains; if mixing intensity is too low, the transition remains above -10°C. Compliance for automotive interior parts requires low volatile organic compound emissions under VDA 278, fogging under DIN 75201 or equivalent OEM standards, and material certification under RoHS Directive 2011/65/EU. End-product types include door panel lower trim, centre console side panels, appliance housings, and battery box covers where processability and dimensional stability of filled PP must be retained. Addition above 20 wt% is not recommended in filled PP because the reduction in flexural modulus can exceed 15% relative to the plastomer-free compound and because surface scratch resistance can deteriorate when the soft phase segregates during mould filling.
Hot-melt adhesive manufacturing with CV77515-F usually positions the plastomer at 15 wt% to 25 wt% of the finished adhesive, with the balance composed of a C5 or hydrogenated hydrocarbon tackifier, a synthetic wax, and a stabilizer package; the plastomer functions as the polymer backbone that raises cohesive strength and low-temperature flexibility without requiring a block copolymer. Compounding in a jacketed sigma-blade mixer or a twin-screw compounder is performed at 150°C to 170°C, with discharge through a heated filtration screen to remove unmelted plastomer particles that otherwise become nozzle-blocking defects in coating heads. Application equipment includes slot-die coaters, spiral-spray nozzles, and roller applicators operating at 150°C to 165°C; open time and set time are adjusted by wax content and plastomer addition rather than by drifting the tank temperature upward, because prolonged holding above 190°C produces char in heated hoses and shifts adhesive viscosity. Regulatory status for food packaging adhesives is governed by FDA 21 CFR 175.105 or EU 10/2011 where the adhesive is not separated from food by a functional barrier; non-food assembly adhesives are evaluated under REACH Regulation (EC) No 1907/2006 and RoHS Directive 2011/65/EU. Viscosity stability is monitored by ASTM D3236 with a Brookfield RVT thermocell at 150°C; ring-and-ball softening point is measured by ASTM E28, and low-temperature adhesion is screened by ASTM D4498 for block shear strength at -20°C. The main failure modes in production are char accumulation in dead zones of melt tanks, viscosity drift from stabilizer depletion during intervals longer than 8 h, and inadequate wet-out on high-gloss carton surfaces when application temperature falls below 150°C. End-product types include case and carton sealing adhesives, bookbinding spine adhesives, packaging lamination, and appliance assembly adhesives where high initial tack and low odour are required.
Crosslinked polyolefin foam producers add CV77515-F at 10 wt% to 30 wt% in LDPE or EVA foam formulations to reduce density, soften the foam into the low Shore C range required for footwear midsoles, and retain cell-wall flexibility at sub-zero temperatures. The mixing sequence on a two-roll mill or internal mixer includes the base polymer, plastomer, azodicarbonamide blowing agent at 5 phr to 15 phr, a peroxide crosslinking agent such as dicumyl peroxide at 0.5 phr to 1.5 phr, and a zinc oxide or zinc stearate kicker; dispersion of the plastomer must be completed before the stock reaches the decomposition onset of the blowing agent to prevent premature gas loss. Press curing is commonly conducted at 160°C to 180°C for 8 min to 15 min, followed by a secondary expansion stage at atmospheric pressure; continuous foaming lines use a hot-air or infrared tunnel at 180°C to 220°C to trigger simultaneous crosslinking and expansion. Gel fraction is measured according to ASTM D2765, with an acceptable range of 40% to 70% for many closed-cell polyolefin foams; compression set is tested under ISO 7214 or ASTM D3575, and density is checked by water displacement. The main process conflict is that the low melting point of the plastomer reduces compound viscosity during the early part of the mixing cycle, which can delay the incorporation of solid blowing agent and produce batch-to-batch density variation. Operators typically adjust mill nip temperature and mixer ram pressure to maintain a cohesive sheet that does not tear at the take-off conveyor. End-product types include athletic shoe midsoles, anti-fatigue mats, gaskets for appliance enclosures, and buoyancy components for marine and sports applications. Compliance is governed by REACH Regulation (EC) No 1907/2006 and RoHS Directive 2011/65/EU; footwear foams additionally require compliance with the brand-specific restricted substance list and California Proposition 65 for certain styrenic or blowing-agent residues where applicable. Published data for CV77515-F in crosslinked foam is limited, so expansion ratio and gel fraction must be confirmed on production-scale mixing equipment rather than extrapolated from unfoamed mechanical data.
Low-voltage cable bedding and jacketing compounds containing CV77515-F are designed around a blend of ethylene-vinyl acetate or LLDPE with alumina trihydrate or magnesium dihydrate at high loadings, with plastomer added at 20 wt% to 40 wt% of the polymer phase to recover elongation and prevent stress cracking after thermal ageing. The compound is prepared on a co-rotating twin-screw extruder with 40:1 L/D and a screw profile that minimizes residence time because the flame-retardant filler can generate local temperature spikes through friable breakdown. Barrel temperatures are set between 140°C and 180°C; the die face is held below 180°C to avoid decomposition of the halogen-free flame-retardant package. The melt is extruded through a cable crosshead at line speeds dependent on conductor diameter, with pressure and melt temperature monitored at the breaker plate; excessive extrusion speed in thin-wall automotive cable can produce cone breaks and surface sharkskin when the plastomer content exceeds 35 wt%. Mechanical properties after extrusion are measured under IEC 60811-501 for tensile strength and elongation at break, while flame propagation is assessed by IEC 60332-1-2 for single cables and thermal stability by IEC 60811-401; automotive road vehicle cables are checked against ISO 6722 for insulation integrity and long-term heat resistance. Environmental compliance requires REACH Regulation (EC) No 1907/2006 and RoHS Directive 2011/65/EU. The plastomer reduces compound modulus and allows higher filler-to-polymer ratios before the elongation falls below 150%, but its lower melting point also reduces the hot-pressure test result if the compound is not crosslinked. End-product types include industrial LV power cables, appliance wiring, automotive thin-wall cables, and photovoltaic junction-box wiring where flexibility and halogen-free flame retardancy are specified. Published data for this specific configuration is limited, and the exact plastomer loading must be tuned against filler type, coupling agent level, and cable standard because filler dispersion and interfacial voids determine long-term insulation resistance.
Competitive Westlake Mxsten® CV77515-F Plastomer prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Westlake Mxsten® CV77515-F Plastomer is an ethylene-1-octene polyolefin plastomer produced through metallocene-catalyzed solution polymerization. The grade is supplied as free-flowing pellets and is used in coextruded sealant films, flexible packaging, polymer impact modification, and selected injection-molded soft-touch components. The manufacturer’s technical bulletin places the material in the low-crystallinity region of the polyolefin spectrum, with a nominal density of 0.875 g/cm³ per ASTM D792 and a nominal melt index of 1.5 g/10 min per ASTM D1238 at 190 °C using a 2.16 kg load. This combination distinguishes the grade from conventional linear low-density polyethylene, which has higher crystallinity, and from high-vinyl-acetate EVA sealants, which may contain a vinyl acetate comonomer that requires venting and can generate acetic acid during thermal degradation.
The metallocene catalyst used in the solution process produces a random 1-octene distribution along the polyethylene backbone and a narrow molecular weight distribution. This architecture suppresses the formation of long crystallizable methylene sequences, thereby lowering the peak melting point and increasing optical clarity. In formulation evaluations, the reduced crystalline content translates into a low secant modulus and a low heat-seal initiation temperature relative to 0.918 g/cm³ LLDPE. Tensile measurements made on ASTM D638 Type IV specimens at 500 mm/min typically show elongation at break values above 800% for the neat resin; however, the producer’s lot-specific datasheet should be consulted because test speed and specimen preparation affect the result. The narrow molecular weight distribution also reduces low-molecular-weight extractables, which is relevant to the organoleptic profile of food-contact films.
Measured haze on a 50 µm cast film typically falls below 5% when the plastomer is used as a neat sealant layer. Gloss at 60° per ASTM D2457 is typically above 80 units. These values are influenced by chill-roll temperature and contact time. The uniform comonomer distribution reduces the scattering centers associated with large crystalline domains, so the optical performance is generally more stable than that of conventional LLDPE after repeated reheating and sealing.
Extrusion processing guidelines for the Mxsten plastomer family recommend single-screw extruders with 24:1 to 30:1 L/D and barrier or Maddock mixing sections. Melt temperatures between 190 °C and 230 °C are established on cast-film lines; blown-film processors sometimes run the plastomer-rich layer at 175–210 °C to avoid bubble instability. On cast-film extrusion, die gap settings between 0.5 mm and 1.0 mm are common, with chill-roll temperatures between 15 °C and 30 °C. Increasing the chill-roll temperature above 30 °C may reduce film flatness because the low crystallinity of the plastomer increases blocking tendency in high-friction surfaces. An antiblock masterbatch is sometimes added at 5–10 wt% in monolayers; in coextruded structures, the plastomer is buried as a sealant to control blocking. Pellets should be kept free of surface moisture in humid plant environments because condensation on cold pellets can cause hopper bridging. Pre-drying is generally not required when the resin is stored in closed original packaging at ambient temperature below 60% relative humidity.
The grade is positioned in the density region between ethylene elastomers and conventional LLDPE. At the stated nominal density of 0.875 g/cm³, the material exhibits a flexural modulus that is less than half the value of a typical 0.918 g/cm³ LLDPE. The lower modulus reduces film crinkle and improves puncture resistance in sealant layers. The heat-seal initiation temperature is commonly evaluated by ASTM F88, with a seal-bar dwell time of 0.5 s and a pressure of 0.28 MPa. In published screening data for similar plastomers, seal strength reaches 4 N/15 mm at temperatures between 90 °C and 105 °C for a 50 µm cast film; however, published data for this specific grade is limited and line-specific sealing windows must be established.
| Property | Test method | CV77515-F typical | EVA 18% VA typical | LLDPE 0.918 typical |
|---|---|---|---|---|
| Density | ASTM D792 | 0.875 g/cm³ | 0.940 g/cm³ | 0.918 g/cm³ |
| Melt index | ASTM D1238 | 1.5 g/10 min | 2.0 g/10 min | 1.0 g/10 min |
| Peak melting point | ASTM D3418 | 55–65 °C | 84–88 °C | 121–124 °C |
| Elongation at break | ASTM D638 | >800% | >600% | >700% |
| Vicat softening | ASTM D1525 | 45–55 °C | 60–65 °C | 95–105 °C |
The table values are screening envelopes from publicly available polymer-class data; they are not contractual limits. For specification-grade comparison, the Westlake technical datasheet for lot acceptance takes precedence.
In high-speed horizontal and vertical form-fill-seal converting, the replacement of EVA is driven by the need to eliminate acetic acid odor, reduce sealant tackiness at the hot-tack test range, and improve toughness at frozen-food temperatures. The lower density of CV77515-F provides wider sealant interdiffusion at temperatures just above the melting onset, but the seal initiation is not necessarily lower than that of a high-vinyl-acetate EVA. Processors often assess hot-tack strength with ASTM F1921 and seal-through-contamination behavior with sachet tests on actual lines. In comparative trials, the plastomer sealant shows higher puncture resistance at -20 °C than an 18% vinyl acetate EVA sealant of equivalent thickness.
Converters should monitor seal-bar temperature uniformity because the plastomer’s narrow melting range produces a rapid seal-strength increase over a narrow temperature interval. The hot-tack window is narrower than that of a fractional-melt LDPE because the plastomer melts over a smaller temperature range. In practice, the seal-bar set point must be controlled within ±5 °C of the validated centerline; otherwise, seal strength drops or film distortion increases. This is especially critical on pouch lines with seal-bar temperature variation across the width above ±3 °C. When the sealant is coextruded with polypropylene or oriented PET, the sealant layer is typically 5–15 µm thick. The sealant layer can be processed at melt temperatures below 230 °C; higher temperatures increase the risk of taste and odor defects, especially if purge times are inadequate. Because CV77515-F contains no acetate groups, purge cycles are generally shorter than those required when changing from EVA to polyethylene.
In impact modification of polypropylene, CV77515-F is metered into a co-rotating twin-screw extruder at 10–30 wt%. The screw configuration should provide distributive mixing before the vacuum vent to avoid local accumulation of low-melting domains. Use of side feeding after the polypropylene melt zone is common because the plastomer pellet viscosity is lower than the polypropylene melt under typical compounding conditions; side feeding reduces screw slippage and melt-temperature gradients. The grade’s low glass-transition temperature improves the ductile-to-brittle transition of heterophasic propylene copolymers in instrumented falling-weight tests following ASTM D3763. This modification route does not require vulcanization or peroxide addition, which distinguishes the plastomer from ethylene-propylene-diene rubber systems.
Within the Mxsten plastomer range, the CV77515-F grade occupies the low-density, moderate-melt-index position. Higher-flow grades in the same family are used where thin-wall injection molding or extrusion coating demands lower viscosity, while lower-melt-index grades are preferred where blown-film melt strength is critical. Compared with the higher-flow grades, CV77515-F provides greater melt strength and better bubble stability; compared with lower-flow grades, it offers more uniform filling in injection molds and higher line-speed capability in cast-film skin layers.
The polyolefin base resin is generally covered by FDA 21 CFR 177.1520(c) for olefin polymers when the finished article meets the specified extractable fraction limitations. European food-contact status is commonly evaluated under EU Regulation No 10/2011, with overall migration limits of 10 mg/dm² for general food simulants. The grade is not formulated with halogenated flame retardants, phthalate plasticizers, or crosslinking agents, and its heavy-metal profile is typically assessed against EU RoHS Directive 2011/65/EU. A supplier-issued declaration of compliance is required for each finished article because additives, converting aids, and coating layers can change the regulatory determination.
| Regulation or standard | Application | Typical confirmatory test or limit |
|---|---|---|
| FDA 21 CFR 177.1520(c) | Olefin polymer food-contact articles | Extractable fraction per 21 CFR 177.1520(d) |
| EU Regulation No 10/2011 | Plastic materials in contact with food | Overall migration 10 mg/dm² |
| EU RoHS Directive 2011/65/EU | Electrical and electronic equipment | Pb, Hg, Cr(VI) threshold 0.1 wt%; Cd 0.01 wt% |
| REACH Regulation (EC) No 1907/2006 | SVHC communication | Article 33 notification if SVHC above 0.1 wt% |
Because final conversion may include printing, lamination, and masterbatch addition, the finished-article compliance must be validated separately from the neat resin.
CV77515-F should not be exposed to sustained service temperatures above 70 °C under constant load, because the low Vicat softening point of the plastomer leads to creep and loss of dimensional stability. It is not recommended for applications requiring continuous contact with aromatic solvents, chlorinated solvents, or mineral-oil-based greases at elevated temperature, since the amorphous phase swells and mechanical properties decline. In melt processing, prolonged residence times above 240 °C or repeated regrind cycles above 30 wt% regrind can increase gel particles and reduce optical clarity. Avoid melt blending with polymers that contain free acidic or strongly oxidizing components, which can accelerate chain scission and shift the seal-performance window.