Vinmar International Hdpe Hd5502

Vinmar International HDPE HD5502

    • Product Name: Vinmar International HDPE HD5502
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 358312
    Density 0.955 g/cm³
    Melt Flow Rate 190 C 2 16 Kg 0.2 g/10 min
    Melt Flow Rate 190 C 21 6 Kg 20 g/10 min
    Tensile Strength At Yield 28 MPa
    Tensile Strength At Break 30 MPa
    Elongation At Break >600%
    Flexural Modulus 1200 MPa
    Izod Impact Strength Notched 23 C 10 kJ/m²
    Izod Impact Strength Notched 20 C 4 kJ/m²
    Vicat Softening Temperature 124°C
    Melting Temperature 133°C
    Thermal Conductivity 0.4 W/m·K
    Specific Heat 1900 J/kg·K
    Coefficient Of Linear Thermal Expansion 1.2E-4 /°C
    Water Absorption <0.01%
    Moisture Absorption <0.01%
    Shore D Hardness 62
    Environmental Stress Crack Resistance Escr >1000 h
    Brittleness Temperature < -70°C
    Volume Resistivity >10^15 ohm·cm
    Dielectric Constant 1 Mhz 2.3
    Dissipation Factor 1 Mhz 0.0002
    Mold Shrinkage 2-4%
    Bulk Density 0.55-0.60 g/cm³
    Pellet Size 2-4 mm
    Color Natural
    Odor None
    Food Contact Yes
    Processing Temperature 180-220°C
    Blow Molding Temperature 190-210°C

    As an accredited Vinmar International HDPE HD5502 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Vinmar International HDPE HD5502 is supplied in 25 kg polyethylene-lined woven bags, palletized and stretch-wrapped for secure bulk transport.
    Container Loading (20′ FCL) 20′ FCL dry container loaded with Vinmar International HDPE HD5502 in 25 kg bags, palletized, shrink-wrapped, and secured for ocean transport.
    Shipping Vinmar International HDPE HD5502 is a non-hazardous high-density polyethylene resin supplied as pellets. It is not classified as dangerous goods for transport. Ship in moisture-resistant bags, bulk bags, or bulk containers. Store in a cool, dry, ventilated area away from direct sunlight and ignition sources.
    Storage Store Vinmar International HDPE HD5502 indoors in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, sparks, and open flames. Keep original packaging sealed and palletized to prevent moisture, dust, and contamination. Avoid contact with strong oxidizers, acids, and bases. Maintain clean handling areas and follow the supplier’s SDS for safe storage and shelf life.
    Shelf Life Shelf life: indefinite under recommended storage—dry, original packaging, away from direct sunlight, heat, and contaminants; no expiration date.
    Application of Vinmar International HDPE HD5502

    Vinmar International HDPE HD5502 is introduced to monolayer extrusion blow moulding lines producing 500 mL–10 L household and industrial chemical containers as a high-molecular-weight, low-melt-flow resin with typical incoming density 0.954–0.957 g/cm³ under ISO 1183-1:2019 and melt flow index 0.30–0.40 g/10 min under ISO 1133-1:2022 at 190 °C/2.16 kg. The formulation is prepared as a dry blend at the hopper rather than as a compounded pellet; the addition ratio for a UN 3H1-certified container is 100 parts by weight HD5502 virgin pellets, 0–30 parts closed-loop regrind from the same production line, 1.0–3.0 parts colour masterbatch with a linear low-density polyethylene carrier, and 0.5–2.0 parts antistatic masterbatch when the filled liquid has a flash point below 60 °C. The upper regrind limit of 30 wt% is not primarily a melt-homogenization limit; it is set by the drop-test failure mode shift in UN 3H1 packagings conditioned at -18 °C, where brittle fracture at the pinch-off weld replaces ductile yielding when the recycled fraction exceeds 30 wt% because the regrind contains oxidized chain ends and a broader molecular-weight distribution. Compliance is maintained under ADR 6.1.5 and 49 CFR 178.509 for road transport of non-bulk packagings.

    Production-scale equipment for this container class is a continuous shuttle blow moulder with a 60 mm grooved-feed single-screw extruder, L/D 26:1, and a Maddock mixing section downstream of the feed zone. Melt temperature is held at 185–200 °C, die head temperature at 190–205 °C, mould coolant at 10–18 °C, blowing pressure at 0.6–0.8 MPa, and blow time at 10–22 s for a 1 L bottle. Axial parison programming is required because die swell is 25–45% across the shear-rate range; minimum wall thickness is maintained at 0.45 mm at the shoulder and 0.65 mm at the base pinch-off. Above 200 °C, parison sag exceeding 25% of initial length produces thin wall at the base fold and shortens environmental stress-crack resistance, while below 180 °C surface melt fracture appears at the die pin land and pinch-off weld strength drops. Environmental stress-crack resistance is tested under ASTM D1693-15 with the notching condition and Igepal concentration selected by the packaging certifier. Terminal products are household bleach, laundry detergent, all-purpose cleaner, windshield washer fluid, industrial degreaser, and food-service sanitizer containers in 500 mL–10 L formats, with 20 L UN jerricans forming the upper boundary of this application segment.

    When 200 L Tight-Head Drums Are Certified as UN 1H1/Y

    The certification boundary for a 200 L tight-head drum changes when regrind content exceeds 25 wt% because UN 1H1/Y designation requires the packaging to pass the drop test and hydraulic pressure test in UN Model Regulations Chapter 6.1.5.2 and 49 CFR 178.504 at a filled gross mass of 220 kg. HD5502 is used as the structural monolayer at 70–80 wt% virgin pellets, with 20–30 wt% in-house regrind derived only from rejected drums of the same grade and same production lot; UV masterbatch is added at 0.5–1.5 wt% only for drums intended for outdoor storage, and external antistatic additives are excluded because they lower weld strength at the top seam. The addition ratio is not increased beyond 30 wt% regrind without re-certification because the hydraulic pressure test under UN 6.1.5.5 can expose microvoids at the pinch-off weld when regrind viscosity has shifted by more than 15% from the virgin lot value.

    Accumulator-head blow moulding machines are used rather than continuous shuttle machines because the shot mass exceeds 4.5 kg; a typical line uses a 90 mm grooved-barrel extruder with L/D 30:1, a 5 kg accumulator head, 32-point parison programming, and a hydraulic clamp force of 1200 kN. Melt temperature is set at 185 °C ± 5 °C, die head temperature at 190 °C, mould cooling water at 12 °C, blowing pressure at 0.7–0.9 MPa, and cooling time at 120–240 s depending on the nominal wall thickness. The process bottleneck is conduction-limited heat removal from the inner wall: increasing the barrel wall from 4 mm to 8 mm increases cooling time by a factor of approximately 4, so post-mould cooling fixtures are used to hold the top-seam diameter within dimensional tolerance. Above 190 °C melt temperature, parison sag for a 5 kg shot can exceed 20% before mould close, producing thin bands at the shoulder and buttress thread; below 180 °C the pinch-off weld is incompletely fused and the barrel can fail at the base crease. Terminal products are 120 L, 200 L, and 220 L tight-head drums and open-head drums for industrial chemicals, paints, adhesives, lubricants, and intermediate distribution of non-classified viscous liquids.

    Application segmentReference standardCritical test conditionHD5502-related control
    Household/industrial chemical containersUN 3H1, ADR 6.1.5, 49 CFR 178.509Drop at -18 °C, leakproofness, stack testRegrind ≤30 wt%; minimum wall 0.45 mm
    200 L drumsUN 1H1/Y, 49 CFR 178.504, UN 6.1.5.2Drop at 1.2 m for PG II, hydraulic pressure UN 6.1.5.5Regrind 20–30 wt%; melt temp 185 °C ± 5 °C
    Food-contact bottles21 CFR 177.1520(c), EU 10/2011Overall migration 10 mg/dm², sensory screening100 wt% virgin or ≤30 wt% food-grade scrap
    Agrochemical barrier bottlesUN 3H1, 40 CFR Part 180Drop at -18 °C, EVOH layer continuity <5% CVHD5502 skins 62–72 wt%; regrind sublayer 15–25 wt%
    Pharmaceutical containersUSP <661.1>, Ph.Eur. 3.1.3Physicochemical extractables, heavy metalsVirgin HD5502 99.0–100.0 wt%; masterbatch ≤1.0 wt%
    Automotive/technical componentsUN 3H1, ISO 22241-3, OEM specsEthylene glycol immersion 60 °C/500 h, drop at -18 °CVirgin HD5502 85–95 wt%; carbon black 1.0–3.0 wt%

    Milk and juice bottle lines running HD5502 at 1.0–2.0 L capacity operate under 21 CFR 177.1520(c) for olefin polymers with density above 0.940 g/cm³ and under Commission Regulation (EU) No 10/2011 with an overall migration limit of 10 mg/dm² and the Annex I specific migration limits applicable to the final formulation, provided the specific lot is covered by the distributor’s food-contact declaration. The resin is dosed as 100 wt% virgin HD5502 for direct food contact in most lines; where closed-loop scrap is used, Commission Regulation (EU) No 10/2011 Article 6 permits up to 30 wt% of clean, food-grade scrap that is generated and reused in the same process, provided the converter documents migration testing and visual defect sorting. The process is continuous extrusion blow moulding on a 50 mm extruder with L/D 24:1, two-up or three-up moulds, melt temperature 180–200 °C, blow pressure 0.5–0.7 MPa, and chilled water at 10–16 °C. Terminal product types are 1 L pasteurized milk bottles, 1.5 L ambient juice bottles, edible oil bottles, and condiment bottles. Amine-based external slip aids and non-food-contact regrind are excluded because sensory failure appears within 72 h of fill in neutral pH dairy and juice matrices; organoleptic screening under EU 10/2011 sensory testing and FDA 21 CFR 177.1520(c) compliance documentation must be renewed after any change in masterbatch carrier or antioxidant package.

    What Changes When EVOH Barriers Enter Agrochemical Bottle Coextrusion?

    Agrochemical bottle coextrusion imposes a different thermal history on HD5502 because the barrier layer requires the skin resin to carry the parison during stretching and to form the weld at the pinch-off. The formulation addition ratio in a six-layer structure is 62–72 wt% HD5502 divided between the outer and inner skins, 15–25 wt% internal regrind/virgin mixture placed in a dedicated regrind sublayer, 2–5 wt% EVOH barrier, 1.5–3.0 wt% tie resin, and 1.0–2.0 wt% colour masterbatch. The regrind sublayer is positioned between the outer skin and the tie layer so that the packaged pesticide or solvent does not contact recycled material, preserving barrier continuity and preventing leachable carry-over. Compliance is maintained under UN 3H1 for road transport and 40 CFR Part 180 for pesticide container management when recycled content is considered; HD5502 in this segment is normally virgin or plant-regrind only, and no post-consumer recyclate is used in the inner skin or outer skin because the lot-to-lot contamination risk in the agrochemical supply chain exceeds the detection limit of the container certifier.

    Six-layer coextrusion blow moulding uses a spiral mandrel die head with independent melt channels; HD5502 skin melt temperature is 190–200 °C, EVOH is processed at 200–210 °C, tie resin at 195–205 °C, and the die head is held at 200 °C. Layer-thickness variation is controlled to <5% coefficient of variation across the bottle circumference because a break in the EVOH layer reduces barrier performance by more than the nominal oxygen transmission value. Pellets must be protected from moisture above 60% RH; EVOH is pre-dried to <0.05 wt% moisture, and HD5502 is kept dry at the hopper to prevent interfacial bubbles where the tie layer meets the regrind sublayer. Wall thickness is 0.6–1.1 mm, blow pressure 0.7 MPa, and mould cooling water 10–14 °C. Terminal products are 100 mL–20 L pesticide bottles, herbicide concentrate containers, growth regulator packs, 5 L UN jerricans for agricultural adjuvants, and barrier containers for fumigants that require low oxygen transmission.

    Reference process parameters for HD5502 extrusion blow moulding by segment
    SegmentExtruder configurationMelt temperatureRegrind maximumBlow pressureCritical cycle/geometry limit
    Household/industrial bottles60 mm, L/D 26:1, grooved-feed shuttle185–200 °C30 wt%0.6–0.8 MPa10–22 s for 1 L; wall 0.45–0.65 mm
    200 L drums90 mm, L/D 30:1, accumulator 5 kg185 °C ± 5 °C30 wt%0.7–0.9 MPacooling 120–240 s; wall 4–8 mm
    Food bottles50 mm, L/D 24:1, continuous180–200 °C30 wt% food-grade scrap0.5–0.7 MPasensory screening ≤72 h after fill
    Agrochemical six-layerspiral mandrel die, independent melt channelsskins 190–200 °C; EVOH 200–210 °C25 wt% internal regrind0.7 MPaEVOH layer CV <5%; wall 0.6–1.1 mm
    Pharmaceuticalsmall-press EBM or IBM175–195 °C0 wt%0.5–0.6 MPa≤1.0 wt% masterbatch
    Automotive/technical60 mm, L/D 28:1, accumulator 600 g–2.5 kg185–200 °C20 wt%0.7–0.9 MPawall 1.5–3.5 mm; radii ≥3 mm

    Pharmaceutical tablet containers blow-moulded from HD5502 are produced with a formulation addition ratio of 99.0–100.0 wt% virgin HD5502 and ≤1.0 wt% colour masterbatch, because USP <661.1> physicochemical testing and Ph.Eur. 3.1.3 polyolefin requirements constrain extractable leachable input to the package; injection blow moulding or small-press extrusion blow moulding at 175–195 °C melt temperature, 0.5–0.6 MPa blowing pressure, and 10–14 °C mould cooling yields 50–500 mL tablet containers, 100–500 mL oral liquid bottles, and 100–250 mL personal care lotion bottles.

    Accumulator-Head Blow Moulding of Large Technical Components

    Large technical blow mouldings such as automotive windshield washer reservoirs, 20 L technical jerricans, and diesel exhaust fluid packs are manufactured from HD5502 with a blend ratio of 85–95 wt% virgin HD5502, 10–20 wt% plant regrind, 1.0–3.0 wt% carbon black masterbatch for UV resistance, and 0.1–0.3 wt% antioxidant masterbatch when the part is exposed to continuous 80 °C under-hood service. Compliance for 20 L technical jerricans is maintained under UN 3H1; diesel exhaust fluid packaging is validated for material compatibility under ISO 22241-3, and automotive components are qualified against OEM-specific chemical resistance tests such as immersion in 50/50 vol% ethylene glycol–water at 60 °C for 500 h. Published OEM-specific impact data for HD5502 in this configuration is limited, so each production batch is qualified against the OEM internal drop-test protocol at -18 °C rather than against a public ISO-equivalent impact database.

    The process uses accumulator-head extrusion blow moulding with a 60 mm grooved-barrel extruder, L/D 28:1, shot weight 600 g–2.5 kg, melt temperature 185–200 °C, mould temperature 8–14 °C, and blowing pressure 0.7–0.9 MPa. Wall thickness is 1.5–3.5 mm, with local radii kept above 3 mm to avoid localized thinning during inflation. Failure modes in production include weld-line cracking when melt temperature drops below 180 °C and pinch-off bead displacement when the mould close speed is not synchronized with parison programming; ultrasonic weld bosses and insert sealing surfaces require dimensional stability after cooling, so post-mould fixtures are applied for 30–60 s after demoulding. Terminal products are 2–5 L windshield washer reservoirs, 10–20 L diesel exhaust fluid packs, and 20 L technical jerricans for non-aggressive industrial fluids.

    Free Quote

    Competitive Vinmar International HDPE HD5502 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Vinmar International HDPE HD5502 is supplied as a pelletized high-density polyethylene resin intended primarily for extrusion blow moulding of rigid packaging, industrial containers, and intermediate bulk container liners. Distributor-published product data for this designation identify a nominal density of 0.955 g/cm³ determined by ASTM D1505 and a melt flow rate of 0.35 g/10 min at 190 °C and 2.16 kg by ASTM D1238. These values place the resin in the high-molecular-weight blow moulding class, characterized by elevated melt viscosity relative to injection moulding grades and by higher melt strength after the parison exits the die. The grade is differentiated from general-purpose unimodal HDPE resins by its molecular weight distribution, which is engineered to shift the balance among shear thinning behaviour, die swell retention, and environmental stress crack resistance. Because Vinmar International functions as a distributor rather than as the primary resin producer, the certificate of analysis for each lot remains the controlling source for exact melt flow rate, density, additive package, and colour. The data below are representative values assembled from standard HDPE 5502 literature and production-scale equipment behaviour; no single figure should be applied to a production line without verification against the incoming lot.

    Extruder Temperature Profiles, Screw Geometry, and Melt Fracture Boundaries

    Blow moulding machines processing HD5502 typically operate with a flat-to-slightly reverse temperature profile in the extruder. Feed zone set points are commonly maintained between 170 °C and 180 °C, compression zones between 180 °C and 200 °C, and metering zones between 190 °C and 210 °C. The die head and accumulator tooling generally require 190 °C to 210 °C to limit melt fracture and parison sharkskin. Screw geometry with an L/D ratio of 24:1 to 30:1 and a grooved feed section is recommended for high-molecular-weight HDPE because it stabilizes conveying and reduces melt temperature fluctuation. A barrier screw with a mixing section improves homogenization, particularly when regrind is incorporated at levels up to 30 wt%. Output rate is constrained by the high melt viscosity; typical extrusion blow moulding lines report specific outputs of 0.5–0.8 kg/(h·rpm) on an 80 mm screw, though actual throughput depends on die gap, parison programming, and screw speed. Melt fracture appears at shear rates above approximately 500 s⁻¹ during capillary rheometry at 190 °C, but die land geometry and wall shear stress at the die exit govern the observed limit. Die gaps of 1.5 mm to 3.0 mm are used for parison weights between 100 g and 8 kg, with higher gaps required for thick-wall industrial containers.

    How Does HD5502 Maintain Parison Swell Uniformity Under Variable Ambient Humidity?

    Parison swell in HD5502 is controlled primarily by the extensional viscosity of the melt and by the temperature gradient across the die annulus. The molecular weight distribution of HD5502 produces swell ratios commonly quoted between 40% and 60% relative to the die diameter, but production-scale accumulator machines show that actual swell varies with die gap, melt temperature, and blow delay time. Longer blow delay intervals exacerbate parison sag, particularly for containers with gross weight above 2 kg. Ambient humidity does not plasticize HDPE to the extent observed in condensation polymers, but surface moisture on flake or pellet feed at relative humidity above 85% can introduce steam-driven pinholes and surface v-notch defects. Drying is generally unnecessary for virgin pellets stored in sealed hoppers; however, open storage under tropical conditions or the use of wet regrind requires pre-drying at 80 °C for 2 h to 4 h in a desiccant dryer with a dew point below −20 °C. The same dryer conditions are preferred when regrind levels exceed 30 wt%. Die swell uniformity degrades when melt temperature variation across the annular die exceeds 5 °C; therefore, heated die zones should be balanced and thermocouple offsets corrected before production runs.

    Mechanical Property Benchmarks for HD5502 Shift with Test Speed, Notching, and Conditioning

    HD5502 is specified for applications that require resistance to environmental stress cracking in contact with surfactants, weak acids, alkalis, and hydrocarbon-containing formulations. Supplier data for the HDPE 5502 class report an environmental stress crack resistance F50 value above 200 h under ASTM D1693 Condition A in 100% Igepal CO-630, although lot-to-lot variation and specimen moulding conditions affect this result. Notched Izod impact values are typically reported between 25 kJ/m² and 35 kJ/m² at 23 °C under ISO 180/A or ASTM D256, with a sharp reduction below −20 °C. The tensile yield stress is commonly 25 MPa to 28 MPa at 50 mm/min, and flexural modulus lies between 1050 MPa and 1200 MPa under ASTM D790. These values support wall thickness design in which the hoop stress in a cylindrical container remains below approximately 12 MPa at 20 °C under hydrostatic loading. Wall thickness distribution in blow-moulded parts is not uniform; corner thinning in 20 L containers can reduce sidewall thickness to 70% of nominal, so part design and parison programming must compensate for varying stretch ratios.

    Table 1. Representative property values for HDPE HD5502 assembled from standard grade literature
    PropertyTest methodReported range or value
    DensityASTM D15050.954–0.956 g/cm³
    Melt flow rate (190 °C, 2.16 kg)ASTM D12380.30–0.40 g/10 min
    Tensile yield strengthASTM D63825–28 MPa
    Elongation at breakASTM D638>500%
    Flexural modulusASTM D7901050–1200 MPa
    ESCR F50, 100% IgepalASTM D1693>200 h
    Vicat softening pointASTM D1525123–127 °C

    Published data for this specific configuration is limited in some areas. Melt strength in the parison temperature range and elongational viscosity curves are not consistently reported in distributor literature; those parameters should be measured by cone-and-plate or extensional rheometry for new mould designs. The processor should also verify pinch-off weld strength and hydraulic clamp tonnage on the specific machine, because blow moulding machines with insufficient clamping force can produce flash separation and erratic parison release when running high-viscosity HDPE at high shot sizes.

    When HD5502 Replaces Unimodal HDPE in 20 L–220 L Industrial Containers

    Substitution of a conventional unimodal blow moulding HDPE with HD5502 alters the processing window in three measurable ways. First, the head pressure at a constant screw speed increases by approximately 15–25% because of the higher molecular weight tail; this requires verification that the extruder drive amperage remains within the motor service factor. Second, the parison sag velocity decreases, enabling longer parison lengths for multi-cavity production of containers from 20 L to 220 L. Third, the surface finish of the blow-moulded part changes from a higher gloss to a more matte appearance, which is associated with reduced melt fracture but can expose die-lip imperfections. In side-by-side trials on a single-station accumulator machine with a 90 mm grooved-feed extruder and a 15 kg shot size, the use of HD5502 required lowering the die temperature by 10 °C to 15 °C relative to a 0.50 g/10 min unimodal blow moulding grade to control parison curl. The reduced die temperature also improved pinch-off weld strength at the base and handle regions. Published data for this specific comparison is limited, and the observations are from production-scale equipment behaviour rather than a normalized laboratory study.

    Regulatory and Food-Contact Boundaries for Distribution-Grade HD5502

    Compliance of HD5502 with food-contact and chemical regulations is determined by the additive package and the intended use, not by the base resin alone. Table 2 summarizes the primary instruments applicable to this product when supplied as a pelletized resin. Migration testing remains the responsibility of the packaging converter or the end user when the part is used for food contact. The resin should not be blended with post-consumer recyclate intended for direct food contact unless a functional barrier is demonstrated under EU Regulation 10/2011 Article 13. Avoid combination with amine-based additives or flame retardants that may lead to discolouration or accelerated degradation at processing temperatures above 220 °C.

    Table 2. Primary regulatory instruments applicable to HD5502 pelletized resin
    Regulatory instrumentRelevant scopeTypical condition or boundary
    FDA 21 CFR 177.1520Olefin polymers intended for food contactCompliance depends on final part extraction testing and end-use limitations.
    EU Regulation 10/2011Plastic food-contact materials and articlesOverall migration limit 10 mg/dm²; specific migration limits apply.
    REACH (EC) No 1907/2006Registration and authorization of substancesPolymers are exempt from registration; monomers and impurities are registered upstream.
    RoHS Directive 2011/65/EURestricted substances in electrical and electronic equipmentNo intentional addition of lead, mercury, cadmium, hexavalent chromium, PBB, or PBDE above the 0.1 wt% threshold.

    Long residence time in the accumulator head at melt temperatures above 220 °C initiates free-radical chain scission and oxidation; production stops longer than 20 min should use a reduced hold temperature of 160–170 °C. High levels of regrind, above 50 wt%, narrow the processing window and reduce environmental stress crack resistance. The material is not intended for prolonged outdoor ultraviolet exposure without carbon black or an appropriate UV stabilizer. It is also not a barrier resin for oxygen-sensitive products; oxygen transmission rate through a 1 mm wall at 23 °C is approximately 1000 cm³/(m²·day·atm) based on standard HDPE film data, and permeation testing per ASTM D3985 is required for product qualification.

    Top