| HS Code | 356420 |
| Polymer Type | High Density Polyethylene (HDPE) |
| Melt Flow Rate | 8.0 g/10 min (190°C/2.16 kg) |
| Density | 0.960 g/cm³ |
| Tensile Stress At Yield | 28 MPa |
| Tensile Strain At Break | >600% |
| Flexural Modulus | 1300 MPa |
| Izod Notched Impact Strength At 23 C | 5 kJ/m² |
| Izod Notched Impact Strength At 20 C | 3 kJ/m² |
| Shore D Hardness | 62 |
| Vicat Softening Temperature | 125°C |
| Heat Deflection Temperature At 0 45 Mpa | 75°C |
| Melting Temperature | 135°C |
| Water Absorption | <0.01% |
| Thermal Conductivity | 0.4 W/m·K |
| Coefficient Of Linear Thermal Expansion | 1.5E-4 /°C |
| Dielectric Constant At 1 Mhz | 2.3 |
| Volume Resistivity | >10^15 ohm·cm |
| Flammability | HB (UL 94) |
As an accredited Versalis HDPE MP 90 PH factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Versalis HDPE MP 90 PH packaging: 25 kg polyethylene bags, palletized and shrink-wrapped for safe storage and transport. |
| Container Loading (20′ FCL) | Versalis HDPE MP 90 PH, in 25 kg bags on pallets, loaded into 20′ FCL containers for secure export shipping. |
| Shipping | Versalis HDPE MP 90 PH is a non-hazardous high-density polyethylene supplied as pellets. It is typically shipped in 25 kg bags, jumbo bags, or bulk trucks/containers. Keep packaging dry, clean, and protected from heat, sunlight, and contamination. Standard industrial transport regulations apply; no dangerous goods classification. |
| Storage | Store Versalis HDPE MP 90 PH in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, ignition sources, and strong oxidizers. Keep original bags closed, on pallets, protected from moisture, dust, and contamination. Avoid excessive stacking or crushing. Do not store outdoors. Keep area clean. Use FIFO and observe supplier shelf-life recommendations. Handle carefully to prevent package damage. |
| Shelf Life | Versalis HDPE MP 90 PH typically has a 24-month shelf life when stored unopened, cool, dry, and away from direct sunlight. |
In potable-water pressure pipe extrusion, Versalis HDPE MP 90 PH is charged at 100 wt% of the monolayer pressure-bearing wall in black pipe formulations, while carbon black masterbatch is let down to a final carbon black concentration of 2.0–2.5 wt% and an antioxidant masterbatch is dosed at 0.2–0.5 wt% to offset thermal history in the extruder. The applicable conformity path for European and Australian water authority approval includes ISO 4427-1:2019 and ISO 4427-2:2019 for polyethylene pressure pipes, EN 12201-1:2011+A1:2018 for drinking water supply, and AS/NZS 4130:2018 for Australian and New Zealand installations. Long-term hydrostatic strength is evaluated under ISO 9080:2012, with classification under ISO 12162:2009 confirming whether the final compound belongs to the PE80 or PE100 MRS band; where supplier documentation does not explicitly state the MRS value for this exact grade, confirmation by an accredited third-party hydrostatic test is required before quoting pressure ratings above PN10. Carbon black content in the pipe wall is checked by ISO 6964:2019, and dispersion is rated under ISO 18553:2002 with a maximum acceptable rating of 3 to avoid localised brittleness and slow crack growth initiation. Extrusion lines for outside diameters from 16 mm to 630 mm typically use single-screw extruders with L/D 30:1–36:1, grooved feed sections, and barrier screws that separate solid-bed transport from melt conveying, with melt temperatures held at 190–220°C and head pressures in the range 15–35 MPa. The processing window is intentionally narrow: below 180°C the viscosity increase raises screw torque and head pressure, producing die-flow instabilities visible as wall-thickness oscillation in the vacuum calibration tank, while above 220°C the antioxidant system is consumed more rapidly and surface oxidation can create gel particles caught by the 80–100 mesh screen pack. The extrudate enters a vacuum sizing sleeve and spray-cooling bath, after which the pipe is cut and conditioned for 24–48 h at 23±2°C before destructive hydrostatic testing. Terminal products include SDR11 and SDR17 potable water mains, industrial process water lines, and geothermal loops rated from PN10 through PN16 where the PE80 or PE100 classification has been verified.
Regrind is excluded from the pressure-bearing wall of gas distribution pipe made from Versalis HDPE MP 90 PH because ISO 4437-1:2020 and EN 1555-1:2021 do not permit recycled or reworked material in the load-bearing layer when rapid crack propagation resistance is required. The standard conversion route uses 100 wt% virgin compound, carbon black masterbatch at a final carbon black concentration of 2.0–2.5 wt%, and an antioxidant masterbatch let-down of 0.2–0.5 wt%; yellow identification stripes are coextruded at 2–5 wt% of total wall thickness using a UV-stabilised HDPE carrier. Extrusion lines run single-screw extruders with L/D 33:1 barrier screws, melt temperature capped at 215°C, and screen-pack filtration at 80–100 mesh to remove micro-gels that act as crack initiation sites. The critical test is ISO 13477:2008, the small-scale steady-state rapid crack propagation test, which propagates an impact crack through a pre-cracked pipe under controlled internal pressure and temperature; the pipe must arrest the crack above maximum operating pressure or the formulation and wall thickness are rejected. Full-scale ISO 13478 RCP testing may also be required by national codes for diameters above 250 mm. Terminal products include PE80 or PE100 gas mains in outside diameters from 20 mm to 400 mm at SDR11 or SDR17.6, distributed through city-gate and district regulator stations, as well as service lines to residential meters.
The −18°C drop test in UN 1H1/1H2 certification is the binding constraint that caps closed-loop regrind in UN-certified jerrycans manufactured from Versalis HDPE MP 90 PH at 20 wt% for non-food industrial chemical packaging. Food-contact versions run 100 wt% virgin resin with a colour masterbatch at 1.0–2.0 wt%; UV stabiliser is added at 0.5–1.0 wt% only where outdoor storage is specified. Compliance references include ADR 6.5, RID 6.5, IMDG Code Chapter 6.5, FDA 21 CFR 177.1520(c), and EU 10/2011 Annex I for food-contact containers. Accumulator-head extrusion blow moulding lines use parison programming with 10–30 point die-gap control, melt temperature 180–210°C, blow pressure 0.6–0.8 MPa, and mould clamping force from 20 t to 100 t depending on container volume. Top-tail pinch-off and flash removal generate trim regrind; any regrind fraction above 20 wt% must be validated under ASTM D1693-15 condition B and the −18°C drop test because each regrind pass raises carbonyl index and shortens the time to stress-crack failure. Closed-loop regrind may be used only when it is clean, of known thermal history, and generated from the same grade; post-consumer recycled material is not permitted in the load-bearing wall. Terminal products include 5–60 L jerrycans for liquid detergents, agrochemical concentrates, and food ingredients, as well as 120–220 L L-ring drums and internal bottles for IBC assemblies.
| Application sector | Primary mandatory reference | Material test method | Pass/fail criterion |
|---|---|---|---|
| Potable water pressure pipe | ISO 4427-1:2019 | ISO 9080:2012 | 20 °C, 50-year hydrostatic strength extrapolation outside 95% lower confidence limit |
| Gas distribution mains | ISO 4437-1:2020 | ISO 13477:2008 | rapid crack propagation arrest above maximum operating pressure |
| UN-certified jerrycans | UN 1H1/1H2 | ASTM D1693-15 Condition B | ESCR failure not permitted before qualification minimum; −18°C drop pass |
| Beverage/pharma closures | FDA 21 CFR 177.1520(c) | EU 10/2011 migration | overall migration ≤ 10 mg/dm² |
| Thermoformed dunnage | ISO 527-3:2018 | IEC 61340-5-1 | surface resistivity ≤ 10^9 Ω/sq where antistatic specified |
| Corrugated drainage/conduit | EN 13476-1:2018 | ISO 18553:2002 | carbon black dispersion rating ≤ 3 |
Versalis HDPE MP 90 PH dosed at 100 wt% in high-speed closure injection moulding is normally combined with a food-grade colour masterbatch at 1.0–2.0 wt%, a slip/anti-block masterbatch at 0.5–1.5 wt%, and a nucleating masterbatch at 0.1–0.3 wt% to stabilise cap roundness after ejection and to reduce differential shrinkage across the tamper-evident band. Compliance for beverage and pharmaceutical closures includes FDA 21 CFR 177.1520(c), EU 10/2011 Annex I with overall migration limited to 10 mg/dm², USP 661.1 for plastic packaging systems, and ISO 8317:2015 for child-resistant closures where specified. The process equipment is a 28–64-cavity hot-runner injection mould with valve-gated tips, melt temperatures at 190–220°C, injection pressure 80–120 MPa, mould temperature 8–12°C, and total cycle time 5–8 s. The shear rate at the sub-gate is high enough to generate flow-induced haze in the cap sidewall if injection velocity is not profiled; process setters therefore ramp velocity in 3–5 steps to avoid jetting and maintain a uniform fill front. Moisture absorbed on cold regrind above 0.05 wt% must be removed with a desiccant hopper dryer at 70–80°C for 1 h when relative humidity exceeds 60%, otherwise splay defects appear on the cap top. Terminal products include 28 mm PCO 1881 beverage closures, child-resistant pharmaceutical bottle caps, tamper-evident bands with break bridges, and snap-on caps for dairy and personal-care containers.
When heavy-gauge sheet is converted from Versalis HDPE MP 90 PH into thermoformed dunnage trays, the formulation is set at 100 wt% virgin resin for food-contact sheet, with post-industrial regrind allowed up to 30 wt% for industrial and logistics applications where food-contact certification is not required. UV-stabiliser masterbatch is dosed at 0.3–0.8 wt% for outdoor pallet top sheets, and an antistatic masterbatch at 1.0–2.0 wt% is used where surface resistivity below 10^9 Ω/sq under IEC 61340-5-1 is specified; published data for this specific grade/antistatic masterbatch combination is limited, so trial validation on the actual flat-die line is required before assigning a guaranteed resistivity range. Sheet extrusion uses a flat die with a polished three-roll stack at 20–60°C, producing sheet thicknesses from 2 mm to 10 mm, followed by plug-assisted thermoforming at draw ratios from 1:1 to 3:1 and mould temperatures of 60–90°C. Above a draw ratio of 3:1, corner thinning exceeds 40% and environmental stress crack resistance in the formed corners becomes the limiting acceptance parameter rather than tensile yield; the relevant mechanical reference is ISO 527-3:2018 for film and sheet, with ASTM D638-14 used where customer specifications demand tensile properties on cut specimens. Terminal products include heavy-duty dunnage trays for automotive parts logistics, pallet top sheets for chemical drums, freezer spacers in food cold-chain handling, and electro-static dissipative trays for electronics assembly.
On corrugated drainage and cable-protection conduit lines, the extruder barrel zones are held at 190–215°C because the moving-mold corrugator draws the melt into thin annular ribs and prolonged residence time accelerates antioxidant loss at high surface-area-to-volume ratios. The compound is charged at 100 wt% virgin Versalis HDPE MP 90 PH, with carbon black masterbatch to final 2.0–2.5 wt% for UV resistance, calcium carbonate at 5–15 wt% where pipe stiffness demands exceed the unfilled modulus, and post-industrial regrind up to 30 wt% with an antioxidant top-up of 0.2–0.5 wt% to compensate for regrind thermal history. Applicable standards include EN 13476-1:2018 for plastic drainage pipes, ASTM F2306/F2306M for corrugated HDPE storm sewer pipe, EN 61386-24 for buried conduit systems, UL 651A for underground HDPE conduit, and CSA C22.2 No. 211.2 for rigid HDPE conduit. Vacuum forming is run at 0.02–0.06 MPa inside the corrugator blocks, the screen pack is 60–80 mesh, and the single-screw extruder has an L/D 30:1 grooved barrel. Carbon black dispersion is checked under ISO 18553:2002 with a maximum rating of 3; poor dispersion creates localised stress concentrations in the corrugation valleys and can produce split ribs during field bending at low temperatures. Terminal products include 50–300 mm double-wall corrugated drainage pipe, UL-listed HDPE electrical conduit, and optical-fiber microduct bundles for telecom trench installation.
Competitive Versalis HDPE MP 90 PH prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Versalis HDPE MP 90 PH is a high-density polyethylene resin supplied as natural pellets and intended for extrusion of pressure pipe, industrial profile, and sheet. Under ISO 1043-1:2011 the material is classified as PE-HD. Manufacturer-issued technical data list a nominal density of 0.953 g/cm³ (ISO 1183-1:2019) and a melt mass-flow rate of 0.45 g/10 min at 190 °C under 5 kg (ISO 1133-1:2022). These values differentiate the grade from injection-moulding HDPE resins with MFR values above 8 g/10 min and from film-grade HDPE with density below 0.945 g/cm³. The specification set is optimized for slow crack growth resistance, high melt strength, and stable pipe wall geometry during calibration.
Published data for this specific configuration is limited in secondary literature; the manufacturer’s technical bulletin and lot certificates should therefore be used as the basis for tooling and extrusion die design. The grade’s broadened molecular weight distribution and high average molecular weight are the primary reasons for its use in solid-wall pipe rather than thin-wall injection-moulded articles. In extrusion trials on single-screw machines, die-pressure fluctuations below ±3% are observed when a melt pump is used after the breaker plate and screw speed is held between 20 rpm and 80 rpm.
Slow crack growth resistance in HDPE pipe is governed by tie-molecule density and the time-dependent disentanglement of high-molecular-weight chains. The molecular architecture of MP 90 PH places short-chain branches preferentially in the high-molecular-weight fraction, which raises the number of load-bearing tie chains without increasing density. Under ISO 9080 hydrostatic stress-rupture testing, pipe grades with this morphology generally show a knee in the stress-time curve beyond 50 years at 20 °C, provided processing-induced defects are absent. The manufacturer’s technical data report an ESCR of F50 > 1000 h under ASTM D1693-15, 100% Igepal CO-630, which is an indicator of resistance to brittle crack propagation in notched specimens. By comparison, a standard unimodal HDPE blow-moulding grade with similar density but narrow molecular weight distribution may exhibit an ESCR below 100 h under the same test method. The notch failure mechanism changes from brittle crack propagation to ductile yielding when tie-molecule density exceeds a material-specific threshold; the bimodal distribution in MP 90 PH is intended to exceed that threshold without increasing the overall density or reducing processability.
Rheologically, the high-molecular-weight tail contributes to a higher zero-shear viscosity and pronounced shear thinning. Capillary rheometry at 190 °C typically shows a power-law index of 0.45–0.55 over shear rates from 10 s⁻¹ to 1000 s⁻¹. This shear thinning enables extrusion through conventional annular dies while retaining melt strength during calibration. The melt elasticity, observed as die swell, is higher than that of a narrow-MWD HDPE with the same MFR; die land length-to-diameter ratios below 8:1 may produce surface melt fracture at outputs above 150 kg/h on 75 mm extruder diameters. Production-scale observations indicate that a screen pack of 60/80/100 mesh and a melt pump downstream of the breaker plate reduce pressure pulsation but do not fully compensate for excessively short die lands.
Substitution of MP 90 PH for a PE100 compound in pressure pipe requires recalculation of wall thickness according to the lower design stress if the grade carries an MRS of 8.0 MPa rather than 10.0 MPa. For a given nominal pressure, wall thickness increases in inverse proportion to the design stress. Designers should use the hydrostatic design basis determined according to ISO 9080 and the material classification under ISO 12162, not nominal density or MFR alone. The grade may be selected for industrial water, irrigation, and drainage lines operating at 20 °C and pressures up to 1.0 MPa, but data for potable-water certification must be obtained from the manufacturer or notified body for each formulation, including carbon black or blue masterbatch. The main advantage of MP 90 PH over lower-molecular-weight pipe grades lies in its higher resistance to slow crack growth after surface scoring or point loading; the trade-off is a lower melt flow rate and higher extrusion torque than MFR 1.0 g/10 min pipe grades.
| Property | MP 90 PH pipe extrusion | HDPE blow moulding | HDPE injection moulding |
|---|---|---|---|
| MFR 190 °C/5 kg (ISO 1133-1:2022) | 0.45 g/10 min | 0.30–0.50 g/10 min | 8–30 g/10 min |
| Density (ISO 1183-1:2019) | 0.953 g/cm³ | 0.945–0.955 g/cm³ | 0.960–0.965 g/cm³ |
| Tensile modulus (ISO 527-2:2012) | 1100 MPa | 900–1000 MPa | 1300–1500 MPa |
| ESCR F50, 100% Igepal (ASTM D1693-15) | >1000 h | 50–200 h | 3–10 h |
| Notched Charpy 23 °C (ISO 179-1) | 20 kJ/m² | 15–25 kJ/m² | 5–10 kJ/m² |
The comparative values are representative ranges for unfilled natural resins; actual commercial grades may vary with comonomer type, additive package, and melt-flow rate. Published data for this specific configuration is limited in secondary sources, and direct substitution should be validated by stress-rupture testing on finished pipe.
Pipe extrusion of MP 90 PH is normally carried out on grooved-barrel single-screw extruders with L/D ratios of 30:1 to 33:1 and a compression ratio of 2.5:1 to 3.0:1. Barrel temperature settings from hopper to die are typically 180 °C, 200 °C, 210 °C, 215 °C, and 210 °C; melt temperature at the die entry is maintained at 210–220 °C. To avoid oxidative degradation that reduces hydrostatic strength, melt temperature should not exceed 225 °C. The die head and adaptor are set 5–10 °C below the final metering zone to increase melt strength before the land. Die land length-to-diameter ratios between 8:1 and 10:1 are used to limit die swell and surface melt fracture. Vacuum calibration tanks are operated at −0.25 bar to −0.60 bar with water temperatures between 15 °C and 25 °C. In practice, a groove-fed extruder with screw diameter of 60 mm may deliver 100–180 kg/h depending on head pressure and cooling capacity. Output is limited less by the resin than by calibration heat transfer; increasing line speed beyond the capacity of the vacuum tank produces out-of-round pipe and residual stress.
Pre-drying is not required when pellet surface moisture is below 0.05 wt%. If storage occurs at relative humidity above 60%, surface condensation can generate splay, microvoids, and internal visible haze in thick walls. In such cases, a dehumidifying hopper set at 80 °C for 2 h is used. Field data from pipe lines indicate that extrusion with carbon black masterbatch at 5–7 wt% lowers melt viscosity slightly and requires a 5 °C reduction in metering zone temperature to avoid over-plasticizing and loss of melt strength.
The process window for MP 90 PH is narrower than for higher-MFR pipe grades. Barrel residence times above 5 min at melt temperatures above 225 °C initiate chain scission and reduce notched slow crack growth performance. Flame-treatment for pipe marking should not exceed an energy density of 45 mJ/cm²; excessive surface oxidation can embrittle the outer skin. The resin should not be blended with polyethylene grades having MFR above 2 g/10 min at levels above 20 wt% if ISO 9080 stress-rupture data are required, because the higher-MFR fraction dilutes the high-molecular-weight tie chains and shifts the ductile-to-brittle transition to shorter times. Additive packages containing free amines or certain phenolic antioxidants at high loadings can interfere with long-term thermal oxidative stability; only formulations prequalified by the producer should be used. Regrind from production scrap may be added at up to 15 wt% in non-critical drainage pipe, but inclusion of degraded film scrap or mixed-color post-consumer recyclate is not recommended without revalidation of hydrostatic strength.
| Regulatory or standard reference | Scope | Status |
|---|---|---|
| REACH (EC 1907/2006) | SVHC and Annex XVII restrictions | Manufacturer declares no SVHC above 0.1 wt% in natural pellet; SDS Section 15. |
| RoHS Directive 2011/65/EU | Cadmium, lead, mercury, Cr(VI), PBB, PBDE | Below restriction thresholds by IEC 62321 screening for natural unfilled resin. |
| FDA 21 CFR 177.1520 | Olefin polymers in contact with food | Natural unpigmented base resin may qualify; final pigmented compound must be reviewed. |
| ISO 12162 | MRS classification | To be verified with manufacturer; design stress is not inferred from density. |
| ISO 9080 | Hydrostatic design basis | Stress-rupture data generated at 20 °C, 60 °C, and 80 °C. |