| HS Code | 588048 |
| Polymer Type | High Density Polyethylene (HDPE) |
| Density | 0.954 g/cm3 |
| Melt Flow Rate 190 C 2 16 Kg | 0.20 g/10 min |
| Tensile Modulus | 1400 MPa |
| Tensile Stress At Yield | 28 MPa |
| Tensile Strain At Yield | 9% |
| Tensile Strain At Break | >600% |
| Charpy Notched Impact Strength 23 C | 10 kJ/m2 |
| Charpy Notched Impact Strength 30 C | 4 kJ/m2 |
| Vicat Softening Temperature | 125°C |
| Shore D Hardness | 65 |
| Environmental Stress Cracking Resistance 10 Igepal | >1000 h |
| Melting Temperature | 134°C |
| Thermal Conductivity | 0.4 W/mK |
| Coefficient Of Linear Thermal Expansion | 1.2E-4 /°C |
| Water Absorption | <0.01% |
| Dielectric Constant | 2.3 |
| Volume Resistivity | >10^16 ohm·cm |
| Processing Temperature | 190-210°C |
| Mould Shrinkage | 2-3% |
As an accredited Versalis HDPE FA 706 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Versalis HDPE FA 706 is packaged in 25 kg PE bags on pallets or 1000 kg bulk bags. |
| Container Loading (20′ FCL) | Versalis HDPE FA 706 loaded in a 20′ FCL container: typically 25 kg bags on pallets, securely stowed for ocean shipment. |
| Shipping | Versalis HDPE FA 706 is shipped as non-hazardous, solid polyethylene pellets. Standard packaging includes 25 kg polyethylene bags, big bags, octabins, or bulk trucks/railcars. Keep dry and away from direct sunlight, heat, and ignition sources. No special transport classification; follow normal industrial handling. |
| Storage | Store Versalis HDPE FA 706 in a cool, dry, well-ventilated area away from direct sunlight, heat, flames, and oxidizing agents. Keep original packaging closed and palletized to prevent moisture, dust, and contamination. Avoid prolonged UV exposure and extreme temperatures. Use appropriate handling to minimize dust and static. Follow supplier SDS and local regulations. |
| Shelf Life | Shelf life: 24 months from production date when stored in original unopened packaging, dry, cool, and protected from direct sunlight. |
Versalis HDPE FA 706 is evaluated downstream for high-melt-strength film extrusion and blow moulding configurations. Injection moulding of thin-wall closures is excluded when the melt flow rate measured under ISO 1133-1:2022 remains below 1.0 g/10 min because filling pressure exceeds conventional machine capability. Unless otherwise stated, pellet moisture should be maintained below 0.05 wt%; material stored above 60% RH should be dried at 80 °C for 2 h in a desiccant dryer to limit surface voids. Each downstream block identifies the applicable compliance instrument, addition ratio, manufacturing method, and terminal article class.
On high-output air-cooled blown film lines with die diameters between 160 mm and 350 mm, Versalis HDPE FA 706 is processed into thin-gauge industrial sack film where film gauge reduction and dart impact resistance are jointly specified. The compliance envelope for this application includes EN 13590:2003 for carrier bags and sacks, EU Regulation 10/2011 when used in food-contact construction, and REACH Annex XVII restrictions for heavy metals if pigmented masterbatch is employed. A recommended addition ratio for a 50 wt% TiO₂ white masterbatch is 3–6 wt%, while a 40 wt% carbon black masterbatch is let down at 1.5–3.0 wt%; slip and antiblock masterbatch is added at 0.5–1.2 wt%, adjusted by film thickness and coefficient of friction targets. The extruder configuration is typically a 30:1–40:1 L/D grooved-feed single-screw extruder with a low-porosity barrier screw, screen pack 20/40/80 mesh, adjustable-lip die gap 1.4–2.0 mm, and dual-lip air ring with internal bubble cooling. Melt temperature measured at the die entrance is held between 205 °C and 230 °C; blow-up ratio ranges from 3.5:1 to 5.0:1. Failure modes observed at the nip include unstable bubble geometry below 1.5 wt% of process aid and edge puckering when frost-line height exceeds 1.5 m. Terminal film thicknesses of 20–80 µm are converted into construction debris sacks, chemical drum liners, pallet over-wrap, and industrial waste sacks. Tensile property verification is performed according to ISO 527-3:2018 and dart impact according to ISO 7765-1:1988.
Household refuse sack conversion places a premium on melt homogeneity and gauge distribution at die diameters above 400 mm. Compliance with EN 13592:2017 for refuse sacks and EN 13430:2004 for material recycling compatibility limits filler and pigment loadings. In monolayer formulations, FA 706 is used as the base resin at 90–98 wt%, with calcium carbonate masterbatch at 2–8 wt% depending on density and opacity targets; the addition of post-consumer recycled HDPE is capped at 20–30 wt% to prevent gel formation and tear-propagation instability. Downstream conversion uses high-speed bottom-seal and lateral-seal lines with accumulation speeds above 200 m/min, start-stop transfer blocks, and differential nip rolls. Process limits observed on converted lines include seal-weld thinning at seal bar temperatures above 165 °C and draw resonance on thin sections below 12 µm when haul-off tension exceeds 0.45 N/mm². Terminal products include star-sealed refuse sacks, drawstring bags with HDPE film, and roll-by-the-meter bin liners.
Because the resin’s high melt strength supports parison hang time, extrusion blow moulding of hazard-class packaging is one of the validated downstream configurations for FA 706. Compliance for UN-designated 3H1 jerrycans of 5–30 L references ADR/RID chapter 6.1, the IMDG Code, and EN ISO 16495:2013. The formulation is processed at 100 wt% virgin resin where full certification is required, or with 10–25 wt% post-consumer recycled HDPE for non-hazardous industrial containers; colour concentrate is metered at 0.5–2.0 wt%, and UV stabiliser masterbatch at 0.2–0.8 wt% for outdoor chemical storage. Production equipment is an accumulator-head blow moulding machine with a shot capacity of 2–10 kg, clamp force between 400 kN and 1000 kN, servo-driven parison programming, and blow-pin calibration. Melt temperature is held at 190–220 °C, mould temperature at 10–25 °C, and blow pressure at 0.6–0.8 MPa. Environmental stress-cracking resistance is verified under ASTM D1693-15e1, and table below gives the verifying test envelope for a packing group II container.
| Verification item | Standard or clause | Applied condition |
|---|---|---|
| Drop impact | ADR/RID 6.1.5.3 | 1.2 m at 23 °C, packing group II |
| Leakproofness | ADR/RID 6.1.5.4 | 20 kPa for 10 min |
| Stacking | ISO 2234:2015 | 40 °C for 24 h |
| Stress-crack resistance | ASTM D1693-15e1 | Condition B, >600 h to failure |
Six-layer coextrusion blow moulding of automotive fuel tanks uses FA 706 in both the outer and inner HDPE layers, with a two-layer regrind structure and a central EVOH barrier. Compliance instruments include ECE R34.02 for fuel tank integrity, CARB LEV III evaporative emission limits, and EPA 40 CFR Part 86.1813 for evaporative emission family standards. The outer layer is compounded with carbon black masterbatch at 0.2–0.5 wt%, tie-resin layers are metered at 1.0–2.0 wt% of the total wall each, EVOH is held at 1.5–3.0 wt% of the total wall, and regrind from trimmed parison flash is reintroduced at 40–50 wt% of the total structure. Processing is conducted on accumulator-head coextrusion blow moulding machines with 5–20 kg shot capacity, servo-driven parison programming, sequential wall-thickness control, and mould temperatures between 10 °C and 25 °C. Melt temperature at the die is maintained between 190 °C and 220 °C; output-rate variations above ±3% can shift EVOH layer thickness beyond ±0.1 mm tolerance, causing permeation failure in emission tests. Published data for this specific FA 706 fuel-tank configuration is limited; tank validation requires full permeability testing on the production tool. Terminal products are 40–90 L multi-layer fuel tanks for passenger vehicles and light commercial vehicles.
Coextruded dry-food liner film on three-layer blown film lines is produced with FA 706 as the high-stiffness core and skin-layer polymer. Food-contact compliance is established under FDA 21 CFR 177.1520, EU Regulation 10/2011, and good manufacturing practice under EC 2023/2006. Layer distribution is set at 15/70/15 or 20/60/20, with FA 706 HDPE layers accounting for 60–80 wt% of the total structure and an LLDPE skin or tie layer at 15–35 wt% for seal initiation and tear reduction; white or opacifying masterbatch is added to the HDPE layer at 2–4 wt%. Processing is carried out on three-layer coextrusion blown film equipment with die diameters between 200 mm and 350 mm, barrier screws in the HDPE extruders, melt temperature of 180–200 °C, and blow-up ratio of 2.5:1 to 3.5:1. Terminal products are cereal liners, cracker liners, and dry snack packaging. High-fat food contact is not recommended without supplemental migration testing because HDPE is not a high-performance oxygen barrier.
Closed-head industrial drum production through accumulator blow moulding requires parison sag resistance over shot weights exceeding 10 kg. For UN-designated 1H1 drums of 120–220 L, the compliance framework includes ADR/RID chapter 6.1, the IMDG Code, and ISO 16104:2011 for the testing of packaging for dangerous goods. The polymer is processed at 100 wt% in natural or pre-compounded formulations; UV-stabilised grades are produced with a UV masterbatch at 1.5–3.0 wt%, antistatic drums for combustible powders incorporate an antistatic masterbatch at 0.5–1.0 wt%, and conductive carbon black formulations are adjusted until surface resistivity falls below 1 × 106 Ω under IEC 60093. Large accumulator-head machines with 10–30 kg shot capacity, two-station shuttle clamps, and servo-parison programming are used. The parison die gap is profiled to compensate for weight distribution, with melt temperature between 190 °C and 210 °C and blow pressure 0.7–0.8 MPa. A recurring failure mode on single-station equipment is weld-line splitting at the pinch-off when the mould flash is too cold, below 15 °C, or when the pinch-off land width is below 2.0 mm. Finished product categories include closed-head chemical drums, solvent containers, and UN-certified export packagings for liquid dangerous goods.
Competitive Versalis HDPE FA 706 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Versalis HDPE FA 706 is a high-molecular-weight high-density polyethylene extrusion grade supplied in pellet form for blown-film and related conversion processes. The product is specified through ISO 1133-1:2022 for melt mass-flow rate, ISO 1183-1:2022 for density, ISO 527-2:2012 for tensile properties, ISO 179-1:2023 for Charpy impact, and ISO 306:2022 for Vicat softening temperature. Representative values reported for the grade include a melt flow rate of 0.7 g/10 min at 190°C/2.16 kg and a density of 0.953 g/cm³. Acceptance decisions should be based on the current Versalis certificate of analysis, because specification limits and typical values may be revised without notice.
The low melt flow rate places the material in the film extrusion class rather than in thin-wall injection moulding. Compared with an injection-moulding HDPE at 8–25 g/10 min, FA 706 produces higher head pressure in grooved-feed extruders and is unsuitable for wall sections below 1.0 mm under standard injection conditions. The same high-molecular-weight fraction that limits injection filling provides the extensional viscosity required to stabilise a blown-film bubble at blow-up ratios from 3:1 to 5:1.
Film-grade high-density polyethylene can be produced with unimodal or bimodal molecular-weight distribution. A bimodal distribution separates the low-molecular-weight fraction that lowers shear viscosity from the high-molecular-weight fraction that increases tie-molecule formation and slow crack growth resistance. This separation permits a melt flow rate of 0.5–0.9 g/10 min to coexist with environmental stress crack resistance values that a simple unimodal resin of equivalent flow often cannot reach. Under ASTM D1693-15, Condition B, 100% Igepal CO-630, high-molecular-weight film grades typically withstand 100 h to 400 h before failure. Published data for FA 706 specifically should be obtained from the manufacturer, because notched ESCR results are sensitive to compression-moulding defects, notch depth, and test temperature.
By contrast, a unimodal film grade with the same melt flow rate may show lower dart impact, lower elongation at break, and earlier mechanical failure at perforation zones during bag conversion. The practical difference appears in high-speed T-shirt bag lines where the film is perforated, folded, and heat-sealed. A resin with lower tie-molecule density can develop pinholes and split propagation at the perforation edge. The exact threshold depends on the final film gauge, blow-up ratio, frost line height, and die-gap geometry, so direct laboratory comparison is preferred over generic grade-class claims.
| Resin class | Melt flow rate (ISO 1133-1:2022, 190°C/2.16 kg) | Density (ISO 1183-1:2022) | Primary processing route | Principal limitation |
|---|---|---|---|---|
| FA 706 / high-molecular-weight film | 0.5–0.9 g/10 min | 0.950–0.956 g/cm³ | blown film | higher backpressure and lower drawdown than injection grades |
| extrusion blow moulding HDPE | 0.2–0.4 g/10 min | 0.949–0.955 g/cm³ | extrusion blow moulding | higher parison sag resistance but increased cycle time and energy demand |
| injection moulding HDPE | 8–25 g/10 min | 0.952–0.960 g/cm³ | thin-wall injection | lower ESCR and insufficient bubble stability for thin blown film |
On a three-layer coextrusion blown-film line, FA 706 is typically processed through a 60–75 mm grooved-barrel extruder with 30:1 L/D. Barrel zone temperatures from feed to metering are commonly 180°C, 200°C, 210°C, 220°C, and 220°C, with adapter and die temperatures maintained at 210–220°C. A screen pack of 60/80/100 mesh is used to protect the die lip. The die gap is set between 1.2 mm and 2.0 mm. A dual-lip air ring with chilled air at 8–15°C supplies primary cooling. Frost line heights below 500 mm can produce residual stress and uneven tear resistance, while heights above 900 mm increase bubble sway under plant air currents. Published data for this specific configuration is limited; the starting conditions are not a substitute for line-specific optimisation.
Below 190°C, the high-molecular-weight tail of the distribution does not fully relax inside the die land. Die-lip shear stress rises, and sharkskin or melt fracture can appear on the outer film surface. The corrective actions are to raise the die temperature to 210°C, reduce screw speed, or add a fluoropolymer processing aid at 0.02–0.05 wt%. When a processing aid is introduced, the die and screen pack require conditioning for 20–60 min before the surface defect clears. Increasing the melt temperature above 230°C is not recommended because high-molecular-weight HDPE oxidises under high shear, producing gel particles and black specks that adhere to the die lip and affect film appearance.
The viscous behaviour of high-molecular-weight HDPE is shear-thinning. At 190°C and an apparent shear rate of 100 s−1, a representative film grade may show shear viscosity between 800 Pa·s and 1200 Pa·s, while at 1000 s−1 the viscosity falls to 200–300 Pa·s. The Arrhenius activation energy for HDPE flow is approximately 25–30 kJ/mol, meaning a 10°C increase in melt temperature reduces viscosity by roughly 10–15%. These values are material-class averages and do not replace capillary rheometry on the actual FA 706 lot.
Injection-moulding trials with FA 706 are not recommended for wall sections below 1.0 mm. The low melt flow rate requires high melt temperature and high holding pressure to fill thin walls, which can degrade the resin and extend cycle time beyond the limits of the application. Published data for this specific configuration is limited.
The onset of sharkskin is controlled by die-land shear stress rather than melt temperature alone. For high-density polyethylene, surface irregularities typically appear when die-land shear stress exceeds approximately 0.14–0.30 MPa, depending on molecular-weight distribution and die geometry. A 1.2 mm die gap at high screw speed can drive shear stress into that range, while a 2.0 mm gap reduces shear stress but also produces a thicker melt layer that may require a higher blow-up ratio to reach final gauge. The operator’s adjustment sequence should therefore begin with die gap and output, followed by temperature, and only then processing aid addition.
Fluoropolymer processing aids work by coating the die land and reducing wall slip. The effectiveness depends on coverage time and the presence of other additives. Amine-based antifog or antistatic masterbatches can interfere with processing-aid coverage and should not be combined with FA 706 unless the additive supplier certifies compatibility. Published data for this specific combination is limited; qualification trials on the actual extrusion line are required.
Application windows for FA 706 include grocery T-shirt bags, freezer film, industrial liners, and courier envelopes. The governing property tests are ASTM D1709-16a for dart drop impact, ASTM D1922-15 for Elmendorf tear, ISO 527-3:2018 for tensile modulus, and ASTM D1003-13 for haze. Testing must be conducted at the final film gauge and with the same machine-direction orientation as production film, because laboratory cast film does not reproduce blown-film orientation.
At a density around 0.953 g/cm³, the grade balances flexural stiffness and moisture vapour barrier. A lower-density film grade near 0.945 g/cm³ may provide higher dart impact but lower tensile modulus and higher water vapour transmission. A blow-moulding HDPE with melt flow rate below 0.4 g/10 min may offer higher parison sag resistance, but it is more difficult to draw down to film gauges below 15 µm. These offsets should be evaluated against the target application rather than assumed from resin class alone.
| Requirement | Reference | Typical condition |
|---|---|---|
| Plastic materials for food contact | FDA 21 CFR 177.1520 | HDPE olefin polymer complying with applicable extractive limits |
| European food contact plastics | EU Regulation 10/2011 | Overall migration and specific migration limits per listed substances |
| REACH SVHC | EC 1907/2006 | No intentionally added substances above 0.1 wt% in the article |
| RoHS hazardous substances | EU 2011/65/EU | Lead, mercury, hexavalent chromium below 0.1 wt%; cadmium below 0.01 wt% |
| Melt flow rate | ISO 1133-1:2022 | 0.5–0.9 g/10 min |
| Density | ISO 1183-1:2022 | 0.950–0.956 g/cm³ |
Storage should avoid direct sunlight and relative humidity above 60%. High-density polyethylene is not hygroscopic, but surface condensation on cold pellets can introduce steam during extrusion and produce bubble defects. Silos and bins should be purged with dry air. Regrind addition should not exceed 10–20 wt% without a full film-gauge and dart-impact requalification, because repeated heat history reduces molecular weight and shifts the film property balance. The resin should not be combined with amine-based antifog or antistatic masterbatches unless the additive supplier certifies that the carrier resin and active package do not cause plate-out, odour, or bubble instability in food-contact films. Published data for this specific combination is limited; qualification trials on the actual conversion line are required.