Versalis Flexirene MR 56 A is processed as a virgin linear low-density polyethylene in rotational moulding lines where the design target is a fully sintered wall of 5 mm to 8 mm without internal cooling channels. Melt mass-flow rate measured under ISO 1133-1:2022 is 5.6 g/10 min at 190 °C/2.16 kg, and density measured under ISO 1183-1:2019 is 0.934 g/cm³. These variables define the practical processing window: the melt must be sufficiently elastic during biaxial rotation to wet the aluminium tool face at 280–310 °C, while the peak internal air temperature must be held at 190–202 °C to prevent micro-void formation at the inner wall. Potable water storage tanks in the 500–15,000 L range are produced on four-arm carousel machines with arm swing diameters from 2,500 mm to 4,500 mm; virgin pellets are first pulverised to a mean particle size of 500 µm (35 mesh) and dry-blended with 1.5–2.5 wt% potable water-grade blue pigment masterbatch. Total non-resin addition is held below 3.0 wt% because higher carrier wax contents in colour concentrates raise the low-temperature impact transition and create brittle failure at 0 °C in the tank base. End-product compliance is governed by NSF/ANSI/CAN 61-2023, EU Directive 2020/2184 Article 11, and UK WRAS BS 6920-1; certification applies only to the moulded article in its final colour and wall thickness, not to the virgin resin. Downstream production uses dry-blend charging, rock-and-roll or biaxial shuttle machines, aluminium moulds with wall thickness 6–8 mm, and forced-air cooling at 8–12 °C/min until the inner wall reaches 80 °C. Demoulding above 90 °C introduces shrinkage marks around threaded outlets. Finished article classes are vertical cylindrical storage tanks, conical-bottom dosing tanks, horizontal transport bowsers, and underground circulation reservoirs.
What Limits Peak Internal Air Temperature in Chemical IBC Inner Bottle Moulding?
Within chemical IBC inner bottle and agricultural dosing tank production, the dry blend is formulated at 96.0–98.0 wt% MR 56 A, 1.5–3.0 wt% carbon black concentrate with a carrier density of 0.920–0.940 g/cm³, and 0.5–1.0 wt% hindered-amine stabiliser masterbatch. Carbon black loading below 1.5 wt% is insufficient for long-term weathering resistance under UN 31H1 exposure requirements, while loading above 3.0 wt% reduces notched Charpy impact at −20 °C to levels that increase drop-test failure. The downstream process operates on closed-loop carousel machines with the primary axis at 3.5–5.0 rpm and secondary axis at 12–16 rpm, approximating a 4:1 rotational ratio. Oven setpoint is 285–305 °C; peak internal air temperature must remain below 205 °C because excursions to 210 °C cause thermal oxidation along the thinnest top-wall regions, visible as yellowing and micro-cracking after 500 h of environmental stress-crack resistance testing under ASTM D1693-21 in 100% Igepal. Finished 1,000 L IBC inner bottles must pass UN Model Regulations Chapter 6.5 design-type tests for rigid plastics IBCs: drop test at 1.2 m for packing group II with a filled relative density of 1.2, leakproofness test at 20 kPa under UN 6.5.6.7, and hydraulic pressure test at 100 kPa for 10 min. Terminal article types include 1,000 L IBC inner bottles, 600–1,500 L horizontal leg tanks, sprayer saddle tanks, and acid dosing stations.
Outdoor Playground Panels and the Low-Temperature Impact Boundary at −15 °C
Outdoor playground component production uses double-wall structural shells with kiss-off ribs to generate local stiffness without increasing overall wall thickness. The dry blend for this segment contains 96.0–97.5 wt% MR 56 A and 2.5–4.0 wt% hindered-amine UV stabiliser masterbatch; the upper limit is critical because decomposition products from excess HALS at processing temperatures above 280 °C migrate to the outer tool face and produce haze. Heavy-metal-free pigments are selected to satisfy EN 71-3:2019+A1:2021 migration limits for barium, cadmium, chromium, lead, arsenic, mercury, antimony, and selenium in accessible toy components. EN 1176-1:2017 and ASTM F1487-21 govern entrapment geometry, head and neck openings, and impact attenuation of playground equipment; the rotomoulded article itself must retain ductile failure in multi-axial puncture testing at −15 °C under ISO 6603-2:2023. Manufacturing is executed on shuttle or carousel machines with cast aluminium tools heated to 270–290 °C; peak internal air temperature is held at 188–195 °C to limit cosmetic sink marks at kiss-off ribs. Cooling is forced air only; water mist is excluded because rapid surface freezing locks in asymmetric crystallinity and produces warpage in panels longer than 1,500 mm. Demoulding proceeds at 70–80 °C with compressed air ejection through corner ports. End products are slide hoods, tunnel segments, climbing panels, roof shelters, and freestanding themed play elements.
Because rotomoulded pallets must combine high impact toughness with steel-insert bonding, the processing sequence begins with pulverised resin at 500 µm mean particle size, dry-blended with 1.0–2.0 wt% colour masterbatch. The formulation is 98.0–99.0 wt% MR 56 A; when pallets enter food or pharmaceutical logistics, all colourants must comply with 21 CFR 177.1520(c) and EU Regulation (EU) No 10/2011 with overall migration below 10 mg/dm². Load-bearing performance is evaluated under ISO 8611-1:2011 racking, stacking, and forklift lifting protocols, while edge impact resistance is assessed with ISO 179-1:2023 Charpy impact at −20 °C. Downstream production uses carousel machines with flat aluminium moulds heated to 280–300 °C, an internal air temperature of 190–198 °C, and a cooling gradient of 5–8 °C/min. The slow cooling segment is retained until steel reinforcing inserts reach 80 °C; demoulding earlier creates radial shrinkage gaps around insert bores and reduces corner drop survival. Terminal articles are export pallets, spill containment decks, drum handling pallets, and cleanroom-compatible transport trays.
When a Rotomoulded Waste Container Must Pass EN 840-1 Drop and Weathering Tests Without Steel Reinforcement
Municipal 660 L and 1,100 L four-wheeled waste containers are produced from a dry blend of 96.0–97.5 wt% MR 56 A, 2.5–4.0 wt% carbon black masterbatch with a melt flow rate of 20–30 g/10 min, and 0.5–1.0 wt% antioxidant/processing stabiliser. The carbon black loading must be at least 2.5 wt% to provide adequate weathering protection under ISO 4892-2 Xenon arc ageing; published data for the exact class-specific exposure time under EN 840-1:2020 is limited and must be confirmed by the moulder. The production method is single-station clamshell rotomoulding with wall thickness of 5–7 mm, oven temperature of 280–300 °C, peak internal air temperature of 190–200 °C, and forced-air cooling to 60 °C before demoulding. Wheel axle inserts and metal reinforcement plates are loaded into the mould before charging; the resin must be pulverised to 500 µm and surface moisture must not exceed 0.05% to avoid steam pinhole defects. End-product performance is validated by EN 840-1:2020 drop tests, ISO 179-1:2023 Charpy impact at −20 °C, and ISO 527-2:2012 tensile yield strength. Terminal articles are municipal waste containers, recycling split bins, and underground lift-bin liners.
Competitive Versalis Flexirene® MR 56 A Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at
+8618005193850
or mail to
sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Versalis Flexirene® MR 56 A Linear Low Density Polyethylene is a pelletized, film-extrusion resin whose commercial identity is defined by two controlled variables: nominal density of 0.926 g/cm³ determined according to ISO 1183-1:2019, and melt mass-flow rate of 1.0 g/10 min determined according to ISO 1133-1:2022 at 190 °C under 2.16 kg. These values place the material in the medium-density segment of the Flexirene linear polyethylene range. The letter sequence MR 56 A is a grade code and does not independently communicate comonomer type, catalyst class, or additive formulation; the manufacturer certificate of analysis and technical data sheet are the controlling documents for lot-specific limits.
Because the polymer is linear and produced by low-pressure coordination polymerisation, it contains short-chain branches introduced by an α-olefin comonomer. The comonomer content is not necessarily disclosed in all public documents; when it is disclosed, it should be treated as a formulation variable rather than a specification limit. The density of 0.926 g/cm³ corresponds to a moderate crystalline fraction. At this density, film made from the resin exhibits higher modulus than a low-density polyethylene of 0.918 g/cm³ and lower modulus than a high-density grade of 0.945 g/cm³. The resulting property balance is relevant to cold-chain packaging, where low-temperature ductility and puncture resistance are required without the high stiffness of HDPE.
The resin is non-hygroscopic. No predrying is required under storage at relative humidity below 60%. If pellets are transferred from cold storage to a warm processing area, condensation can form on the pellet surface; in that case a dehumidified drying step at 60–80 °C for 2–4 h is standard practice. The grade is not normally UV-stabilised unless a specific variant is ordered; films intended for permanent outdoor exposure require additional stabiliser masterbatch.
Primary specification variables and test methods
| Variable |
Normative method |
Controlled value or condition |
| Density |
ISO 1183-1:2019 |
0.926 g/cm³ |
| Melt mass-flow rate |
ISO 1133-1:2022 |
1.0 g/10 min at 190 °C/2.16 kg |
| Antioxidant stabilisation |
Internal quality control |
Present; package varies by end-use grade |
| Moisture control |
Internal quality control |
Non-hygroscopic; surface condensation only |
Rheological and Thermal Boundaries in Blown-Film Conversion
Blown-film lines used for this product are typically single-screw extruders with L/D ratios of 24:1 to 30:1 and barrier screws or mixing sections for melt homogenisation. Melt temperature is normally set between 195 °C and 230 °C. The lower boundary is controlled by screw torque and melt pressure; the upper boundary is controlled by gel formation and oxidative degradation. In a linear low-density resin, viscous heating can raise melt temperature by 10–15 °C above barrel set point at high screw speed, so barrel set points are not equivalent to true melt temperature. Die pressure on a 55 mm, 30:1 extruder running at 80–120 kg/h is commonly reported in the range 200–350 bar for butene-based linear film grades. For MR 56 A, the specific pressure should be logged on the production line because it depends on die gap, screen-pack condition, and melt filtration.
Bubble stability is the primary process conflict because linear grades lack the long-chain branching of high-pressure LDPE. The converter should begin with a die gap of 1.8–2.5 mm and a blow-up ratio in the range 2.0:1 to 3.0:1. Lower blow-up ratios reduce bubble flutter but tend to shift tear balance toward machine direction. Frost-line height is adjusted using air-ring and internal bubble cooling. If internal bubble cooling is installed, it is used above roughly 150 kg/h; lack of internal cooling at high outputs may push the frost line upward and produce haze bands. The thermal boundary at 240 °C should be treated as a maximum short-term melt-temperature excursion. Prolonged operation above 260 °C risks additive degradation and gel contamination.
Production-scale failure modes observed with linear grades in this viscosity range include screen-pack pressure rise, die lip deposit, and bubble instability near the frost line. Screen-pack pressure rise is usually caused by unmelted material or crosslinked gels generated during high-temperature excursions. Die lip deposit can occur when the additive package is not matched to the die-lip shear rate. Bubble instability is exacerbated by non-uniform air-ring flow and plant air turbulence; corrective actions include lowering the frost line, increasing die gap, or reducing blow-up ratio. Cast-film conversion is possible but process demands differ. In cast film, the linear structure produces more neck-in than high-pressure LDPE but less than some higher-flow linear grades. Air-knife position and die-to-chill-roll distance are set to stabilise the web. Because the melt-flow rate is low for injection moulding, the product is not recommended for high-flow moulding.
Compared with high-pressure low-density polyethylene, MR 56 A has higher tensile strength and dart impact at the same film gauge, but lower melt strength and usually lower gloss. In the melt state, the zero-shear viscosity of a high-pressure LDPE at the same melt index is usually lower than that of a linear low-density grade, but the branched LDPE has a strain-hardening response in extensional flow. MR 56 A, lacking long-chain branching, does not exhibit the same degree of extensional strain hardening. This molecular distinction allows the linear grade to be drawn down to thinner gauges under appropriate conditions, but requires tighter control of the bubble.
Against high-density polyethylene, MR 56 A offers lower stiffness and lower heat resistance but substantially better low-temperature ductility and environmental stress-crack resistance. The higher permeability to oxygen and water vapour must be compensated by barrier layers in packaging structures where shelf life is limiting. Within the Flexirene family, higher-density grades in the 0.930–0.940 g/cm³ range are used where stiffness and temperature resistance outweigh impact; lower-density grades in the 0.918–0.922 g/cm³ range provide lower seal initiation and higher hot tack. MR 56 A occupies an intermediate position. The choice of MR 56 A over a lower-density grade usually reflects the need to down-gauge a film while retaining tensile stiffness; the choice against a higher-density grade often reflects cold-chain impact requirements or reduced risk of stress cracking.
Qualitative differentiation from adjacent polymer families
| Reference resin |
MR 56 A relative behaviour |
Method by which the difference is normally quantified |
| High-pressure LDPE |
Higher shear viscosity, lower melt strength |
ISO 11443:2021 capillary rheometry |
| HDPE |
Lower density, lower crystallinity, lower stiffness |
ISO 178:2019 flexural modulus and ISO 11357-3:2018 crystallinity |
| C8-LLDPE |
Lower dart impact and tear resistance at the same density |
ASTM D1709/A falling dart and ISO 6383-2:1983 Elmendorf tear |
The comparison against C8-LLDPE is dependent on comonomer type. If the MR 56 A public datasheet does not identify the comonomer, the difference in tear and dart impact cannot be assumed from density alone; a film trial using the same die and frost line is required. The grade should not be substituted into a metallocene-C8 film structure without first comparing heat-seal curves and dart impact at the target gauge.
How Do Food-Contact and Industrial Regulatory Frameworks Apply to MR 56 A?
Food-contact status is not an intrinsic property of the resin. The base olefin polymer may be formulated to meet FDA 21 CFR §177.1520 for olefin polymers and EU Regulation (EU) No 10/2011 for plastic materials and articles. However, the finished film must be evaluated with the exact additive package and processing aids. Under EU 10/2011, the overall migration limit is 10 mg/dm²; specific migration limits for additives and oxidation products are listed in the regulation and must be checked against the resin manufacturer’s declaration of compliance. Under FDA 21 CFR §177.1520, the polymer may be used as a component of food-contact articles provided that the final article meets extractives limitations and any applicable end-use conditions.
On the industrial side, the resin is subject to REACH (EC) No 1907/2006 registration. The converter should confirm that the supplied registration covers the intended end use and that any substance of very high concern is not present above the communication threshold of 0.1% w/w. For medical packaging or pharmaceutical containers, additional assessment under ISO 10993-1:2018 and USP Chapter 661.1 is required for the final component. These standards do not grant a blanket approval from the resin grade alone. Batch traceability from the resin lot to the finished film lot is required because food-contact compliance is a supply-chain document set, not a physical property.
When Low Seal Initiation Temperature and Puncture Resistance Are Both Critical
In frozen-food packaging, bag-in-box liners, and collation shrink film, the seal layer must develop seal strength quickly at a temperature low enough to avoid damaging contaminated film. MR 56 A is used in these structures because its density of 0.926 g/cm³ provides lower seal initiation than HDPE and better hot-tack than high-pressure LDPE in many converters’ line trials. Seal performance is not specified by a single datasheet value; it is mapped by producing heat-seal curves according to ASTM F1921 and seal-strength tests according to ASTM F88. Typical seal initiation values for this density class are lower than comparable HDPE but higher than very-low-density ethylene copolymers; the exact curve shifts with comonomer content, slip additives, and seal bar configuration.
The grade is also positioned in the core layer of heavy-duty films where dart impact and tear resistance are primary. On three-layer coextrusion lines with die gaps of 1.8–2.5 mm, MR 56 A is frequently blended with 10–30 wt% high-pressure LDPE. The LDPE addition improves bubble stability and drawdown but reduces clarity and dart impact. The optimum blend ratio is line-specific; a fixed ratio cannot be specified across all die diameters and cooling geometries. Published data for this specific configuration is limited, so the blend ratio must be established by film trial with the actual extruder screw and die.
Surface-treated film made from MR 56 A can be printed or laminated after corona treatment at discharge levels measured by ASTM D2578-23 for wetting tension. Corona levels must be matched to the ink or adhesive system; excessive treatment can create polar low-molecular-weight species that interfere with seal strength. The material is not recommended for continuous service above 80 °C in structural applications because of its thermoplastic softening range, and it should not be combined with incompatible high-acid or chlorinated polymer residues in the same extrusion system without purging.