| HS Code | 972909 |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene |
| Density | 0.923 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 0.6 g/10 min |
| Melting Point | 122 °C |
| Vicat Softening Temperature | 100 °C |
| Tensile Strength At Yield | 11 MPa |
| Tensile Strength At Break | 30 MPa |
| Elongation At Break | 800% |
| Flexural Modulus | 260 MPa |
| Dart Drop Impact | 150 g |
| Elmendorf Tear Resistance Md | 110 g |
| Elmendorf Tear Resistance Td | 220 g |
| Haze | 14% |
| Gloss 45 | 55% |
As an accredited Versalis Flexirene® FH 56 A Butene Copolymer Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Versalis Flexirene® FH 56 A is supplied in 25 kg polyethylene bags, palletized and stretch-wrapped; 1,000 kg bulk bags are also available. |
| Container Loading (20′ FCL) | Versalis Flexirene® FH 56 A Butene Copolymer Linear Low Density Polyethylene, 25 kg bags, palletized and secured in a 20′ FCL. |
| Shipping | Versalis Flexirene® FH 56 A is shipped as non-hazardous polyethylene pellets in 25 kg bags, 500–1000 kg FIBCs, or bulk tankers/railcars. Not classified as dangerous goods. Keep containers closed, dry, cool, and out of direct sunlight. Avoid moisture, contamination, and ignition sources. Follow local regulations and the SDS. |
| Storage | Store in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep containers or bags closed to prevent moisture, dust, and contamination. Use original packaging, stack securely, and avoid prolonged exposure to high temperatures or oxidizing agents. Store at moderate temperatures, preferably below 40°C. Follow local regulations and supplier instructions. |
| Shelf Life | No specific shelf life; stable for years if stored cool, dry, in original packaging, away from sunlight and contaminants. |
In 120 µm to 180 µm heavy-duty industrial sacks for hot-filled polymer granules, calcium chloride pellets, and regrind, FH 56 A is run on grooved-feed single-screw extruders with a 30:1 L/D barrier screw and a Maddock mixing section, typically of 60 mm to 75 mm diameter. The melt temperature is held between 195 °C and 210 °C at the die entry, the die gap is set at 1.8 mm to 2.5 mm, and the blow-up ratio is limited to 2.0 to 3.0 unless the line is fitted with internal bubble cooling; above 3.4 BUR the low-melt-tension butene copolymer exhibits bubble flutter and gauge spread wider than ±15% at the frost line. Frost line height is controlled at 6 to 8 die diameters. Output on a 60 mm extruder is typically 70 kg/h to 95 kg/h at a head pressure of 180 bar to 240 bar; when head pressure exceeds 250 bar, the screen pack is reduced from 60/80/100 mesh to 40/60/80 mesh to limit solids accumulation. Dart drop tested under ASTM D1709-24 Method A on 150 µm film is used as the lot-release criterion; a target of 280 g to 350 g is obtained at 2.8 BUR when the film is cooled at an air ring temperature of 10 °C to 18 °C. Tensile strength under ISO 527-3:2018 Type 5 at 200 mm/min normally exceeds 35 MPa MD and 25 MPa TD, but the anisotropy is governed by frost line height rather than die gap. An LDPE grade with a melt index of 0.3 g/10 min is added at 15 wt% to 25 wt% to overcome bubble instability during gauge transitions from 80 µm to 180 µm. For sacks that must retain contents at -20 °C, the addition of more than 20 wt% LDPE lowers dart drop, so the structure is coextruded with a pure FH 56 A core and an LDPE skin at 12% of total thickness. Seal strength of 150 µm film tested under ASTM F88/F88M-21 at 150 °C, 0.3 MPa, 1 s dwell should exceed 40 N/15 mm when the heat-seal layer is 100% FH 56 A.
| Test standard | Specimen or condition | Application limit |
|---|---|---|
| ISO 1133-1:2022 | 190 °C/2.16 kg | Lot acceptance 0.72 g/10 min to 0.88 g/10 min |
| ISO 1183-1:2019 | 23 °C immersion | Nominal 0.921 g/cm³ |
| ASTM D1709-24 Method A | 150 µm film, 38.1 mm dart | 280 g to 350 g at 2.8 BUR |
| ISO 527-3:2018 | Type 5, 200 mm/min | MD ≥35 MPa, TD ≥25 MPa |
| ASTM D1922-23 | Elmendorf tear, 150 µm | TD ≥12 N/mm |
| ASTM F88/F88M-21 | 150 °C, 0.3 MPa, 1 s | ≥40 N/15 mm |
Agricultural clamp sheets of 150 µm to 200 µm thickness are produced from the same grade on 90 mm grooved-feed blown-film lines with 2.2 m die circumference, where the formulation is 92% FH 56 A, 5% LDPE, 2.5% carbon black masterbatch, and 0.5% hindered amine light stabiliser masterbatch. Silage juice resistance is monitored by tensile retention after 30 days immersion in 2 wt% lactic acid at 40 °C under ISO 175:2010; retention above 80% is required before the lot is released. Puncture resistance measured by ISO 14477:2010 at 300 mm/min on 180 µm film is specified at not less than 500 N, a value that constrains frost line height to 5 to 7 die diameters because higher frost lines reduce crystallinity and puncture energy. The film is welded at 190 °C and 0.4 MPa for 2.5 s to produce 18 m x 12 m clamp covers; weld failure under ISO 527-3:2018 Type 5 must occur in the film body rather than the weld line. For black-white coextruded structures, the white skin is 15 µm of a metallocene LLDPE and the black layer is 165 µm of FH 56 A; this configuration keeps surface temperature under 35 °C when exposed to 900 W/m² solar irradiance for 4 h, measured with a black-globe thermometer. Batch-to-batch variation in dart drop under ASTM D1709-24 Method A is controlled within 15% by specifying the supplier’s lot MFR range of 0.72 g/10 min to 0.88 g/10 min under ISO 1133-1:2022. If the sheet is intended for clamp silage in areas with wind gusts above 100 km/h, the edge anchoring system is reinforced with woven polypropylene bands and the film gauge is increased to 220 µm; published data for this specific configuration is limited.
For extrusion lamination onto aluminium foil 9 µm to 20 µm for desiccant sachets, the melt temperature at the die lip is maintained at 290 °C to 310 °C, not because of adhesion but because lower temperatures increase the melt curtain width fluctuation and unstable wave patterns at the laminating nip. The polymer is blended with 20 wt% to 30 wt% LDPE of 0.92 g/cm³ density to reduce neck-in from 80 mm to 45 mm at a 200 mm die gap and a 18 mm die-to-nip distance. Line speeds of 80 m/min to 150 m/min are used; above 150 m/min the extensional viscosity of FH 56 A butene copolymer triggers draw resonance that appears as alternating thick-thin bands parallel to the coating width. Coating grammage is set at 15 g/m² to 25 g/m²; at grammage below 12 g/m² pinhole count under ASTM D5151-19 exceeds 2 per m² on foil, which disqualifies the laminate for barrier sachets. Adhesion to foil is generated after the aluminium substrate is chemically primed with a titanium-modified organic complex, and adhesion measured under ASTM F88/F88M-21 must exceed 2.5 N/15 mm at 180 °C seal bar temperature, 0.3 MPa pressure, 0.5 s dwell. Hot tack at 130 °C to 150 °C is tested using ASTM F1921-23; the blended coating retains 1.5 N/25 mm to 2.5 N/25 mm at 0.08 s cool time. The process window narrows when quartz-coated rubber nip rolls are used because FH 56 A sticks above 60 ppm moisture on the roll surface; roll temperature is held at 15 °C to 20 °C. The terminal sachet punctures at 18 N to 22 N under ISO 14477:2010. Food-contact status for the sachet film is evaluated under EU 10/2011/EC migration testing and FDA 21 CFR 177.1520 conditions, not by resin grade alone. No additional primer is needed on the polyethylene side for heat sealing against a 40 g/m² paper layer.
Flat-weave polypropylene sack lamination uses FH 56 A at 18 g/m² to 22 g/m² applied directly onto corona-treated woven fabric at 40 kW/m² intensity; the hot melt web is drawn from a 250 mm slot die and pressed by a water-cooled silicone rubber roll at 18 °C to 22 °C and 35 N/mm nip pressure. Line speed is restricted to 90 m/min to 120 m/min because the low melt strength of the butene copolymer produces edge weave at higher speeds. The coated fabric is converted into 50 kg fertiliser sacks, and adhesion to the polypropylene fabric is tested by a 180° peel method at 300 mm/min, with a requirement above 6 N/15 mm. Because the web contains low slip additive loading, the coefficient of friction under ASTM D1894-24 on the coated exterior is 0.35 to 0.45 at 23 °C; sacks stacked 4 high on a pallet at 1000 kg load show no sliding when the pallet is inclined at 18°.
For 25 µm to 40 µm cast surface-protection film applied to cold-rolled steel coils, FH 56 A is processed at 220 °C to 240 °C on a 75 mm/70 mm two-layer cast line with a 0.5 mm die lip and a chill roll temperature of 25 °C to 30 °C. The film is coextruded with a 10 µm adhesive layer of low-molecular-weight polyolefin; the backing layer consists of 60 wt% virgin FH 56 A and 40 wt% post-industrial regrind from edge trim and roll splices. Regrind level above 40 wt% reduces the tensile modulus below 140 MPa and increases the gel count above 40 gels per 500 cm², causing localised black specks in the adhesive interface and release ghosting after 8 weeks of outdoor storage. Elongation at break under ISO 527-3:2018 must remain above 400% MD to allow the coil to be unspooled without film fracturing at 90° bend radii. The film is expected to release with a peel force between 0.8 N/25 mm and 2.0 N/25 mm under ASTM D3330/D3330M-23 Test Method F at 180° and 300 mm/min; this range is maintained by limiting the chill roll temperature to 25 °C ± 2 °C because lower quench temperatures increase the amorphous layer thickness and raise peel force. When coils are stored at 50 °C black surface temperature for 30 days, the film must not delaminate from the coil edge; this requirement excludes formulations with recycled content exceeding 60%. The terminal protected coil is flat-rolled without oil traces because the film contains no migratory ester plasticiser; the absence of residues is verified by wiping with isopropanol and inspecting under UV at 365 nm.
Carbon black masterbatch for polyolefin pipe uses FH 56 A at 40 wt% carbon black loading in a co-rotating twin-screw extruder at 200 °C to 220 °C, with an additional acid scavenger at 0.15 wt% when the supplier stabiliser package is insufficient for the compounding residence time.
Competitive Versalis Flexirene® FH 56 A Butene Copolymer Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Versalis Flexirene FH 56 A is a butene copolymer linear low density polyethylene supplied as a pelletised base resin for blown film conversion. The product is produced through gas-phase polymerisation with a Ziegler-Natta catalyst system; 1-butene is incorporated as the short-chain branching comonomer. Manufacturer-published nominal density is 0.921 g/cm³ according to ISO 1183-1, and melt mass-flow rate is 1.0 g/10 min measured at 190 °C under 2.16 kg load according to ISO 1133-1. The molecular architecture therefore contains predominantly linear polyethylene chains with ethyl branches, distinguishing the grade from homopolymer HDPE and from long-chain branched high-pressure LDPE.
The base grade carries an antioxidant stabilisation package. Slip agents, antiblock agents, fluoropolymer processing aids, and UV stabilisers are not intrinsic to the grade designation unless specifically declared in the certificate of analysis. Converters that require controlled coefficient of friction, high corona retention, or tailored blocking behaviour should treat these as downstream formulation variables rather than properties of the as-supplied pellet.
| Property | Nominal value | Test method or source |
|---|---|---|
| Density | 0.921 g/cm³ | ISO 1183-1 |
| Melt mass-flow rate | 1.0 g/10 min | ISO 1133-1, 190 °C, 2.16 kg |
| Comonomer | 1-butene | FTIR or 13C NMR |
| Stabilisation | Antioxidant package | Supplier certificate of analysis |
| Slip or antiblock | Not intrinsic to base grade | Supplier certificate of analysis |
For food-contact applications, the olefin polymer baseline described in 21 CFR 177.1520 may apply, but finished-article compliance, migration limits, and specific conditions of use must be established through supplier documentation and the relevant national or European regulation. Under REACH, the safety data sheet should be confirmed for registration status, SVHC content below 0.1% w/w, and any use restrictions applicable to the supplied grade.
On a 65 mm single-screw blown-film line with an L/D of 30:1, spiral mandrel die, and die gap between 1.5 mm and 2.0 mm, the resin is normally processed in the melt-temperature range of 180 °C to 210 °C. The optimum profile is equipment-dependent: higher barrel temperatures reduce extruder pressure and improve melt homogeneity, but excessive melt temperature lowers bubble stability and increases oxidation risk at long residence times. A blow-up ratio of 2.0:1 to 3.0:1 is representative for the density and melt-flow envelope of FH 56 A; within this window, frost line position has a greater influence on tear balance than does the exact die temperature. Frost line heights from 250 mm to 500 mm are used in standard LLDPE film production to shift the balance between machine-direction and transverse-direction orientation. The short-chain branching content of FH 56 A contributes to strain-hardening behaviour that is lower than high-pressure LDPE but sufficient for stable bubble operation when air ring and internal bubble cooling are balanced.
Bubble stability in LLDPE blown film is controlled by the deformation-hardening behaviour of the melt as it passes the frost line. The ethyl branches derived from 1-butene depress the crystallisation rate relative to HDPE, while the broad molecular weight distribution of a Ziegler-Natta butene LLDPE provides shear-thinning behaviour that can reduce die pressure and improve melt homogeneity at moderate screw speeds. At a 2.5:1 blow-up ratio, the primary risk is not melt fracture at the die lip but bubble sag between the die and the frost line. The lower melt strength of FH 56 A relative to high-pressure LDPE means that high-stalk configurations, where the bubble is intentionally elongated before expansion, require either a lower melt temperature or LDPE addition to prevent instability. Blending 15 wt% to 30 wt% of low-melt-index high-pressure LDPE raises extensional viscosity and stabilises the bubble; the exact addition level is a function of die geometry, ambient air temperature, and target gauge.
The molecular weight distribution also affects the onset of sharkskin. Because the grade has a melt index of 1.0 g/10 min, melt fracture is less likely at a given shear rate than in fractional-MFI grades. If the die gap is below 1.0 mm or output rates exceed the resin’s critical shear stress, a fluoropolymer processing aid is required rather than a temperature increase alone. Published data for this specific configuration is limited; critical shear stress should be determined on the conversion line.
Distinction from metallocene and octene-based LLDPE is not limited to comonomer cost or morphology. FH 56 A contains a broader interchain comonomer distribution, with some chains carrying high short-chain branching content and others carrying low short-chain branching content. This produces a broader melting range and slower optical clarity development than metallocene LLDPE of the same density. Compared with octene-based LLDPE, the butene branch is shorter; at equal density and MFR, a butene resin tends to exhibit lower dart impact and tear strength but also lower extrusion pressure. The following table compares product classes on relevant blown-film attributes.
| Resin class | Comonomer | Branch length | Blown-film bubble stability | Dart impact at equal gauge | Haze without clarifying additives |
|---|---|---|---|---|---|
| Flexirene FH 56 A | 1-butene | Ethyl | Moderate; LDPE blending often used | Moderate | Higher than mLLDPE |
| Ziegler-Natta octene LLDPE | 1-octene | Hexyl | Comparable or slightly better | Higher | Comparable to moderately hazy |
| Metallocene LLDPE | 1-hexene or 1-octene | Butyl or hexyl | Lower melt strength; narrower MWD increases die pressure | Higher at reduced gauge | Lower |
| High-pressure LDPE | None | Long-chain branching | High melt strength; best for high-stalk operations | Lower | High-clarity grades available |
Downgauging FH 56 A below 30 µm on high-stalk equipment introduces competing limitations. The low melt strength of the butene LLDPE requires a shorter frost line or a lower melt temperature to reduce gravitational sag, but lowering the melt temperature narrows the processing window for haze control and raises the risk of gel formation from high-molecular-weight fractions. On a 40 mm grooved-feed extruder with a 1.2 mm die gap, attempts to run below 25 µm without LDPE can lead to bubble flicker and a reduction in dart impact measured by ASTM D1709 Method A. Increasing the blow-up ratio above 3.0:1 may improve transverse-direction tear but also intensifies instability because the longer polymer path increases residence time in the unstabilised molten bubble surface. In such configurations, 20 wt% to 30 wt% of a 0.3 g/10 min high-pressure LDPE is generally required to restore bubble stability and maintain gauge uniformity. The exact addition level must be established on the target line, because air ring type, internal bubble cooling capacity, and die diameter shift the limit.
Published data for this specific configuration is limited; therefore, the downgauging limit is not a resin property but an equipment-dependent response. Converters evaluating FH 56 A in such operations should use a design of experiments that includes melt temperature, frost line height, blow-up ratio, and LDPE content rather than a single supplier recommendation.
In extrusion, the shear viscosity of FH 56 A is intermediate between a high-pressure LDPE and a fractional-MFI linear resin. The melt index of 1.0 g/10 min means that die pressure in a standard blown-film die can be controlled without excessive screw torque on extruders with L/D ratios up to 30:1. For cast film or sheet lines, the process temperature window can be shifted upward, but residence times above 230 °C should be limited to prevent oxidative degradation of the antioxidant package. Amine-based additives are not categorically incompatible with this polyethylene grade, but their interaction with phenolic stabilisers and silicone release agents should be evaluated by accelerated ageing, because amine chemistry may interfere with the long-term thermal stabilisation mechanism. Fluoropolymer processing aids are often used at 400 ppm to 800 ppm to delay sharkskin in narrow die gaps or high-output operations; these levels are additive additions and do not represent a property of the base resin.
For cast film and sheet extrusion, the resin can be used when the cooling roll configuration is set for lower melt strength; however, edge neck-in is higher than with high-pressure LDPE, and the melt may require a lower air gap. For injection moulding and rotational moulding, the grade is not optimised; the melt index and molecular structure are designed for film extrusion rather than long-flow moulding. Converting the product into thin-wall injection-moulded articles would require a higher melt flow grade to avoid short shots at typical moulding clamp force limits of 80 t to 150 t. Published data for this specific configuration is limited, and suitability must be confirmed on the target conversion line.