| HS Code | 924935 |
| Polymertype | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene-1 |
| Density | 0.923 g/cm³ |
| Meltflowrate | 0.8 g/10 min (190°C/2.16 kg) |
| Meltingpoint | 124 °C |
| Vicatsofteningtemperature | 100 °C (1 kg) |
| Tensilestrengthatyield | 11 MPa |
| Tensilestrengthatbreak | 30 MPa |
| Elongationatbreak | 700 % |
| Flexuralmodulus | 250 MPa |
| Shoredhardness | 50 |
| Thermalstability | Antioxidant stabilized |
As an accredited Versalis Flexirene® FG 23 F Butene Copolymer Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Versalis Flexirene FG 23 F is typically supplied in 25 kg polyethylene bags, palletized and stretch-wrapped, with 1,000 kg bulk bags available. |
| Container Loading (20′ FCL) | 20′ FCL: Versalis Flexirene FG 23 F LLDPE butene copolymer in 25 kg bags, palletized, shrink-wrapped, typically 18–22 MT total. |
| Shipping | Versalis Flexirene® FG 23 F Butene Copolymer LLDPE ships as non-hazardous solid resin pellets. Standard packaging includes 25 kg bags, bulk bags, or bulk containers, palletized and shrink-wrapped. Transport by road, rail, sea, or air under dry, clean conditions; no dangerous-goods placards required. Store away from heat and moisture. |
| Storage | Store in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep original packaging closed to prevent moisture and contamination. Avoid contact with strong oxidizing agents. Do not stack excessively high. Protect from UV and dust. Ensure containers are labeled and sealed when not in use. Use good housekeeping and first-in, first-out stock rotation. |
| Shelf Life | Recommended shelf life is 24 months when stored in original packaging, cool, dry, well-ventilated area, away from direct sunlight. |
On three-layer blown film lines equipped with internal bubble cooling and 30:1 L/D grooved-feed extruders, Flexirene FG 23 F is introduced as the core layer linear backbone at 50–70 parts by weight per 100 parts of polymer, with a low-density polyethylene fraction of 20–40 parts and colour masterbatch in an LDPE carrier at 5–10 parts. The grade is characterised by melt flow rate under ISO 1133-1:2022 at 190 °C/2.16 kg, with density measured under ISO 1183-1. Outer layers carry antiblock concentrate based on diatomaceous silica at 1–2 parts and erucamide slip at 500–1,500 ppm of total compound, while the core layer may receive 5–15 parts recycled trim from in-line slit edges. For industrial sack production, melt temperature is held between 195 °C and 215 °C, die gap is set to 1.4–2.0 mm, and blow-up ratio is limited to 2.5–3.2 to maintain dart impact resistance in the machine direction. The film is drawn through a collapsing frame with fibre battens, and edge trim is fed back to the core layer at controlled ratios to limit gel formation. Regulatory compliance for non-food industrial packaging uses REACH Regulation (EC) No 1907/2006 and, for packaging heavy metals, EU Directive 94/62/EC with sum concentration limits for lead, cadmium, mercury, and hexavalent chromium below 100 mg/kg. Terminal products include form-fill-seal heavy-duty sacks for petrochemical resins, mineral fillers, and construction powders, with thicknesses from 100 µm to 200 µm, as well as welded gusseted liners for FIBC antistatic overpacks. Tensile yield and elongation are monitored by ISO 527-3 on 15 mm punched specimens, and Elmendorf tear is measured according to ISO 6383-2; film line output and frost line height must be revalidated per gauge.
In cast stretch film lines with 45 mm or 65 mm single-screw extruders and polished chill rolls maintained at 18–24 °C, Flexirene FG 23 F is combined with a metallocene-catalyzed linear low-density polyethylene fraction to set the stiffness-elastomer balance. The butene resin is charged at 30–50 parts by weight per 100 parts of polymer, the metallocene LLDPE at 50–70 parts, and polyisobutylene cling agent at 1.0–2.5 parts per 100 parts of polymer. The molten web exits a coat-hanger flat die with lip opening 0.8–1.2 mm, is quenched on a matte or polished chill roll, and is edged through a vacuum box to limit neck-in before slitting to 750 mm rolls. The oxygen transmission rate is measured by ISO 15105-2 on 25 µm film to determine whether the finished wrap meets the silage fermentation specification; because butene comonomer produces wider interlamellar spacing than octene under equivalent cooling, the measured value must be checked against the target before downgauging. Compliance for silage film is assessed under EN 13207:2018 for silage thermoplastic films, including thickness tolerance and tear resistance, and under REACH Regulation (EC) No 1907/2006 for substances of very high concern. Terminal product types are cylindrical bale wraps in 25 µm and 30 µm gauges, pre-stretched hand rolls, and combined net-wrap replacement films for round balers. Line operators record chill roll motor load and winder tension because butene LLDPE with cling agent can exhibit winding telescoping when roll hardness exceeds 85 shore C.
Where heat-seal integrity after flex-cracking is the primary specification, Flexirene FG 23 F is run as the sealant layer in three-layer blown film structures at 80–100 parts by weight per 100 parts of polymer, with a low-density polyethylene modifier at 0–20 parts and a processing aid at 400–800 ppm of total compound to suppress melt fracture. The sealant web is produced on water-cooled blown film lines with 1.2–1.8 mm die gaps, melt temperatures of 185–205 °C, and blow-up ratios of 2.0–2.8; the collapsing frame is set low to minimise blocking. For lamination to biaxially oriented polyester or aluminium foil, the film is corona-treated in-line to 38–42 mN/m as measured by ASTM D2578, then adhesive-laminated on a solventless laminator at 1.5–2.5 g/m² adhesive coat weight. Food-contact compliance is established under FDA 21 CFR § 177.1520(c) for olefin polymers and EU Regulation (EU) No 10/2011 with an overall migration limit of 10 mg/dm² under the specified simulant conditions; compliance statements must list the exact grade lot and conversion temperatures because heat-seal initiation shifts with film density and die-line history. Terminal product types include frozen vegetable pouches, dry soup sachets, snack laminates, and condiment stick packs, with sealant layer thicknesses of 30–60 µm. Heat-seal strength after lamination is measured by ASTM F88/F88M on 25.4 mm strips; a target sealant layer value above 12 N/25 mm at 130 °C seal bar temperature is commonly used for high-speed vertical form-fill-seal packing, though the specific sealant layer thickness and dwell time must be validated on the target machine.
For 150–200 µm three-layer greenhouse covers, Flexirene FG 23 F is placed in the external layers at 70–90 parts by weight per 100 parts of the external layer compound, with low-density polyethylene at 10–30 parts; the middle layer contains ethylene-vinyl acetate at 10–20 parts and the butene resin at 30–50 parts, plus hindered amine light stabilizer masterbatch at 0.8–1.5 parts per 100 parts of total film compound. The external layers are extruded at 190–210 °C through a 1.8–2.4 mm die gap, and the bubble is stabilised at a blow-up ratio of 2.0–2.8 with a frost line height of 400–600 mm above the die; the butene linear fraction controls dart impact and puncture resistance, but alone does not provide multi-year UV ageing performance, so the stabiliser package must be increased for high-UV sites. Compliance is assessed according to EN 13206:2017 for thermoplastic films for agricultural and horticultural use, and REACH Regulation (EC) No 1907/2006 for UV stabiliser migration and disposal declarations. Terminal films include single-season low tunnels, three-season greenhouse cladding, and thermal screen support layers, with widths up to 16 m on collapsing frames with central gussets. Puncture resistance of the finished greenhouse cover is measured by EN ISO 12236, and retention of tensile elongation after photo-ageing is checked by ISO 4892-2 in xenon arc chambers; published data for this specific butene grade in multi-year outdoor roofing configurations is limited, so field validation at local solar irradiance is required for warranty-backed installations.
As blown film orientation moves from low-stalk to high-stalk conditions, Flexirene FG 23 F is added at 30–40 parts by weight per 100 parts of polymer blend, with high-pressure LDPE at 50–60 parts and the remaining balance adjusted to control machine-direction orientation. The film is produced on blown film lines configured for high-stalk or low-stalk bubble stability, with die diameter 250–400 mm, die gap 1.6–2.2 mm, blow-up ratio 3.5–4.5, and frost line height adjusted within 250–450 mm to set the balance between transverse and machine direction shrink. After primary tube collapse, the film is annealed on heated rolls at 70–90 °C and slitted to multipack widths from 400 mm to 1,200 mm. Shrinkage is tested in hot oil or hot air according to ASTM D2732, and shrink force is measured by ASTM D2838 on 25.4 mm strips, with tunnel oversize specified against a 0.8 N/cm target; the butene LLDPE fraction reduces the onset of melt holes at tunnel temperatures above 170 °C but requires a slip package to prevent blocking. Compliance is limited to non-food industrial packaging under REACH Regulation (EC) No 1907/2006 and, for export to North America, CONEG heavy metal limits for packaging. Terminal products include shrink-wrapped bottled water multipacks, canned goods trays, and stationery bundles at thicknesses of 45–90 µm.
Temporary protective film for high-gloss metal cladding imposes a different set of surface chemistry constraints that eliminate erucamide slip and favour a low-migration formulation. Flexirene FG 23 F is used as the backing layer at 70–90 parts by weight per 100 parts of polymer phase, with a polyolefin elastomer at 10–30 parts to reduce modulus and an antiblock masterbatch based on synthetic silica at 0.5–1.0 parts per 100 parts of polymer phase; no primary amide slip agent is added because migrating amides can transfer to adhered stainless steel or anodised aluminium surfaces. The film is cast through a 1.0–1.4 mm lip gap onto a polished chill roll at 20–28 °C, with line speeds between 80 m/min and 150 m/min, and is corona-treated to 36–40 mN/m on the adhesive-bearing side before transfer coating of a solvent-free acrylic adhesive at 10–20 g/m². Regulatory compliance is managed under REACH Regulation (EC) No 1907/2006 for industrial use, with product safety declarations aligned to RoHS Directive 2011/65/EU where the protected article is an electrical appliance housing; the polymer itself is not in food contact but the adhesive system requires separate food-contact migration testing where the tape is applied to food-processing equipment surfaces. Terminal product types are temporary protective films for stainless steel sheet, pre-painted aluminium profiles, polycarbonate glazing panels, and coated metal cladding, with backing thicknesses from 40 µm to 80 µm and peel adhesion values measured by ASTM D3330 between 0.5 N/25 mm and 3.0 N/25 mm. Because butene LLDPE backings show stress relaxation under sustained winding tension, roll storage is specified below 35 °C to avoid telescoping and adhesive transfer at the edges.
Competitive Versalis Flexirene® FG 23 F Butene Copolymer Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Versalis Flexirene® FG 23 F is a butene copolymer linear low density polyethylene supplied in pellet form for blown film extrusion. The grade is produced with a nominal melt flow rate of 2.3 g/10 min when measured at 190 °C under 2.16 kg load in accordance with ISO 1133-1:2022. Nominal density is 0.923 g/cm³ determined by ISO 1183-1:2019 method A on compression-moulded specimens. These two indicators place FG 23 F in the medium melt-flow segment of the Flexirene range, between lower-flow blown film grades with higher melt strength and higher-flow grades intended for thin-gauge or high-speed extrusion. The comonomer is 1-butene, which introduces short-chain branches along the linear ethylene backbone. That molecular architecture reduces crystallite thickness and lowers the crystalline melting point relative to high-density polyethylene, while retaining the processability and cost structure of a butene-copolymerised LLDPE.
| Parameter | Test method / designation | Unit | Nominal value |
|---|---|---|---|
| Melt flow rate | ISO 1133-1:2022 condition T | g/10 min | 2.3 |
| Density | ISO 1183-1:2019 method A | g/cm³ | 0.923 |
| Comonomer | — | — | 1-butene |
| Physical form | — | — | Cylindrical pellets |
For engineering calculations, the mass-flow melt flow rate can be converted to melt volume-flow rate using the melt-density convention of 0.7632 g/cm³ applied in standard melt flow instrumentation. The resulting nominal melt volume-flow rate is approximately 3.01 cm³/10 min. This parameter is more relevant than mass flow rate when evaluating die-head throughput, shear rate, and screw recovery characteristics in film extrusion.
Butene-derived short-chain branches are excluded from the crystalline lattice of linear low density polyethylene. The resulting lamellar thickness distribution broadens the melting endotherm and shifts the crystallization point to a lower temperature than that of a high-density polyethylene of comparable melt flow. In blown film processing, this affects frost line position and the development of transverse direction orientation. Compared with shorter or absent branch architectures, the butene comonomer yields a lower lamellar perfection and a lower density, which generally increases elongation and impact absorption while reducing tensile modulus.
The rheological response of FG 23 F is characterised by a comparatively low degree of shear thinning relative to high-pressure LDPE. The absence of long-chain branching reduces melt extension hardening and makes the bubble more sensitive to changes in air ring flow, die gap, and frost line height. Capillary rheometry is required before die design calculations. Published data for this specific configuration is limited, and the grade should not be assumed to follow the power-law parameters of a general-purpose butene LLDPE without confirmation on a production-scale capillary viscometer or torque rheometer.
Solid-state properties should be assessed on film rather than on moulded plaques. Tensile properties are normally measured under ISO 527-3 using 25 mm-wide film strips at a test speed of 500 mm/min. Secant modulus at 1% strain is determined under ASTM D882. Dart drop impact is evaluated by ISO 7765-1 method A or ASTM D1709. Elmendorf tear resistance is measured in machine and transverse directions according to ISO 6383-2 or ASTM D1922. Haze and clarity are measured with ISO 14782 and gloss with ISO 2813 at 60°. Film property values are strongly dependent on gauge, blow-up ratio, frost line height, extrusion temperature, and additivation; datasheet values therefore require confirmation on the intended production line before package design finalisation.
When FG 23 F is processed on single-screw extruders with grooved feed sections and 24:1 to 30:1 L/D, the resin is typically introduced using a barrier screw or a Maddock mixing section to disperse thermal stabiliser and optional processing aids. Screen packs of 40/60/80 mesh are commonly used, although the final pack depends on melt pressure limitations. Rear zone temperatures are generally set in the range of 170 °C to 190 °C, with front zones and adapter sections from 200 °C to 230 °C. Die temperatures are held between 210 °C and 230 °C on many blown film lines. Melt temperature should remain below 250 °C to limit thermo-oxidative chain scission and gel formation during extended runs.
Film gauge reduction below 30 µm intensifies the melt strength demands on the resin. FG 23 F can be down-gauged, but bubble stability becomes sensitive to the ratio of blow-up ratio to longitudinal draw ratio. High-stalk lines that produce a long melt cone above the die require controlled strain hardening to prevent bubble oscillation and draw resonance. Because FG 23 F is linear and lacks long-chain branching, its stabilising mechanism depends more on cooling rate control than on extensional viscosity. Frost line height should be maintained within a narrow band; excursions of 50 mm or more can generate gauge variation and visible haze differences across the film roll.
On low-stalk air-cooled dies, the risk of unstable freeze line movement is reduced, but the optical properties may decline if the melt cools too slowly. The crystallisation rate of the butene copolymer is lower than that of HDPE, so a longer residence time in the partially molten state permits thicker lamellae formation and can increase film haze. Rapid quenching with an internal bubble cooling system or high-velocity air ring can mitigate this effect. Excessive head pressure and localised melt temperature spikes can promote melt fracture and sharkskin at the die exit. In such conditions, a fluoroelastomer polymer processing aid may be added at the recommended dosage to delay the critical shear stress for surface defects.
For blends, small additions of 10 wt% to 20 wt% high-pressure LDPE are frequently used to improve bubble stability and transverse direction tear balance. The addition of LDPE modifies the rheological signature by introducing long-chain branching and reduces the tendency for splitty film behaviour in high blow-up-ratio production. The exact blend ratio should be determined by the final film gauge and required dart impact. Higher LDPE content increases bubble stability but reduces tensile strength and puncture resistance, so the formulation should be tested against the end-use specification.
The principal differentiation of FG 23 F from LDPE is the absence of long-chain branching. High-pressure LDPE exhibits higher melt extension hardening and broader bubble stability under high blow-up ratios, but lower tensile properties at equivalent gauge. FG 23 F provides better downgauging potential in applications where tensile strength and puncture resistance dominate, provided the line has sufficient cooling and tension control. Compared with high-density polyethylene film grades, FG 23 F has lower stiffness and higher dart impact energy, making it more suitable for flexible packaging rather than rigid overwrap requiring high modulus.
Within the Flexirene family, adjacent grades differ mainly in density and melt flow. Lower-density butene LLDPE grades such as Flexirene FG 20 F offer higher elongation and lower modulus at equivalent gauge, while higher-flow grades such as Flexirene FG 30 F offer reduced melt pressure and higher throughput on small die diameters but lower bubble stability. FG 23 F is positioned where a balance of thin-gauge mechanical performance, processability, and sealability is required.
Compared with hexene and octene LLDPE grades of similar density and melt flow, the butene comonomer in FG 23 F generally produces lower dart impact, lower Elmendorf tear, and lower hot-tack strength. Hexene and octene copolymers create longer short-chain branches that are more effective at forming tie-chain populations between lamellae. The selection between butene, hexene, and octene grades is therefore driven by the required toughness and seal performance at a given cost threshold. In applications where dart impact on 25 µm film is the limiting specification, a hexene or octene grade may be technically preferred; where the specification allows butene-level toughness, FG 23 F can be processed without the higher cost of longer comonomer grades.
Regulatory suitability should be confirmed on the final article. Polyethylene grades of this class are commonly assessed according to EU Regulation (EU) No 10/2011 for plastic food contact materials and under FDA 21 CFR 177.1520 for olefin polymers. The final overall migration limit of 10 mg/dm² applies to the food contact article, not to the resin alone, and is dependent on the concentration and type of masterbatches, processing aids, and layer structure. Specific migration of 1-butene and any auxiliary additives must be evaluated under the intended food simulant and time-temperature conditions. Under REACH, the polymer itself is exempt from registration, while ethylene and 1-butene monomers are subject to registration obligations and exposure scenario evaluation. Packaging waste compliance is assessed on the final packaging article under Directive 94/62/EC heavy metal concentration limits, and the converter should verify that pigments or printing inks do not introduce regulated heavy metals above the threshold.
Storage should be conducted in closed packaging away from direct sunlight and prolonged exposure to moisture. Pre-drying is not normally required if packaging is intact and ambient relative humidity is below 60%. If pellets are stored in humid conditions or exposed to condensation, surface moisture can generate film defects and reduce adhesion. Purging with low-density polyethylene or a commercial purging compound is recommended between product changeovers to avoid gel accumulation in the die. The resin should not be exposed to prolonged heating above 250 °C; degradation at elevated temperature produces low-molecular-weight fractions that can increase extractables and alter seal strength.
On injection moulding and cast film equipment, FG 23 F is not typically the first-choice grade because its molecular weight and comonomer structure are optimised for blown film bubble stability. Cast film lines may experience edge neck-in and draw resonance unless the blend or line speed is adjusted. Film produced from FG 23 F should be conditioned at 23 °C ± 2 °C and 50% ± 5% relative humidity for at least 40 h in accordance with ISO 291 before mechanical testing, because semicrystalline polyethylene film properties drift during post-extrusion crystallisation.