| HS Code | 238252 |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene-1 |
| Density Typical | 0.920 g/cm³ |
| Melt Flow Rate 190c 2 16kg Typical | 1.0 g/10 min |
| Melting Point Typical | 122 °C |
| Vicat Softening Temperature Typical | 95 °C |
| Tensile Strength At Yield Typical | 10 MPa |
| Tensile Strength At Break Typical | 30 MPa |
| Elongation At Break Typical | 800% |
| Tensile Modulus Typical | 200 MPa |
| Dart Drop Impact Typical | 120 g |
| Haze Typical | 12% |
| Gloss Typical | 60% |
| Form | Pellets |
| Color | Natural |
As an accredited Versalis Flexirene® FG 20 U Butene Copolymer Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Versalis Flexirene® FG 20 U is supplied in 25 kg polyethylene bags, palletized and stretch-wrapped, with 55 bags per pallet (1,375 kg). |
| Container Loading (20′ FCL) | 20′ FCL loading for Versalis Flexirene FG 20 U: 18 pallets, 55 × 25 kg bags each, 24.75 MT net. |
| Shipping | Versalis Flexirene® FG 20 U is shipped as non-hazardous, solid polyethylene pellets in sealed moisture-barrier bags—typically 25 kg sacks or 500–1000 kg jumbo bags on pallets. Transport in clean, dry trucks/containers; avoid heat, direct sunlight, and contamination. No special UN/DG classification. Store sealed in dry, ventilated conditions. |
| Storage | Store Versalis Flexirene® FG 20 U Butene Copolymer LLDPE in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and oxidizing agents. Keep original bags/containers closed, off the floor, and protected from moisture, dust, and contamination. Avoid prolonged UV exposure. Use FIFO stock rotation, maintain good housekeeping, do not stack excessively, and follow the manufacturer’s safety data sheet. |
| Shelf Life | Shelf life is typically 24 months from production when stored unopened, dry, below 40°C, away from direct sunlight and heat sources. |
On monolayer blown film towers equipped with dual-lip air rings, internal bubble cooling, and die diameters of 250–400 mm, Flexirene FG 20 U is run at melt temperatures of 185–210 °C with a die gap of 1.8–2.2 mm and blow-up ratio of 2.5:1–3.5:1. The grade’s nominal density of 0.920 g/cm³ and melt flow rate of 1.0 g/10 min at 190 °C/2.16 kg under ISO 1133-1 define a process in which bubble instability, not extruder torque, is the first limit on output; blending 10–20 wt% LDPE with melt flow rate 0.3–0.5 g/10 min at 190 °C/2.16 kg raises melt pressure at the breaker plate by 10–20 bar on a 25:1 L/D single-screw extruder but permits higher take-up speed without collapsing the frost line. Compliance for industrial liners and heavy-duty shipping sacks is governed by REACH (EC) No 1907/2006; the article is not intended for food contact and does not require migration testing. Addition ratios for this segment are 75–90 wt% Flexirene FG 20 U, 10–20 wt% LDPE for melt strength and bubble morphology, and 2.5–5.0 wt% carbon black masterbatch where outdoor opacity or UV screening is specified. The downstream process maintains gauge variation within ±8% via segmented die control and capacitive thickness scanning across web widths up to 1,800 mm. Terminal articles are 100–200 µm heavy-duty shipping sacks, 80–150 µm construction temporary containment films, pallet covers, and industrial liners for non-hazardous bulk goods. A known failure mode in this butene copolymer is machine-direction tear propagation measured by ISO 6383-2, which falls below hexene and octene LLDPE at equivalent density; converters therefore avoid gauges below 60 µm when tear resistance is specified.
In three-layer coextruded food-contact structures where heat-seal initiation must remain below 105 °C, Flexirene FG 20 U is introduced in the sealant layer as 65–85 wt% of that layer’s blend, with 10–25 wt% LDPE for bubble stability and 5–15 wt% plastomer only when contaminated or cold-seal performance is required. Food-contact compliance is verified under EU 10/2011 Annex I with an overall migration limit of 10 mg/dm² across food simulants and under FDA 21 CFR 177.1520 for olefin polymers; finished-article compliance is formulation-dependent and requires supplier migration documentation for slip and antiblock masterbatches. The conversion route is blown film coextrusion with die gap 1.6–2.0 mm, BUR 2.0:1–2.8:1, melt temperature 185–210 °C, and either internal bubble cooling or dual-lip air ring. Heat-seal curves generated according to ASTM F88 at 50 N/cm² jaw pressure and 0.5 s dwell time show that adding 5 wt% plastomer shifts seal initiation downward by 5–10 °C relative to the unmodified grade; coefficient of friction is measured according to ASTM D1894 after 48 h maturation because primary amide slip agents such as erucamide require 24–72 h to migrate and reduce surface COF to specification. Terminal articles are 25–70 µm bag-in-box liners, frozen food pouches, dairy powder liners, and bakery film. An operational boundary is in-line conversion: film packed or sealed before slip migration completes can exhibit surface coefficient of friction above the 0.20 target and block in roll storage.
Silage and greenhouse cover conversion combines low-temperature toughness with ultraviolet stabilizer dispersion; Flexirene FG 20 U is used at 80–95 wt% with 5–15 wt% LDPE and 5–8 wt% HALS/UV masterbatch to deliver 0.6–1.2 wt% active hindered amine light stabilizer in the final film. Compliance for crop covering is verified under EC No 1907/2006 REACH and EN 13206:2017 for thermoplastic agricultural covering films; no food-contact migration assessment is required under this use. The blown film process uses three-layer towers with die diameter 350–600 mm, die gap 1.8–2.4 mm, BUR 2.0:1–3.0:1, and melt temperature 190–215 °C; HALS masterbatch is pre-dried at 60–70 °C for 2 h when silo storage relative humidity exceeds 60% to prevent hydrolysis of carrier resin moisture. A measurable process conflict emerges above 8 wt% HALS masterbatch: viscosity mismatch between the masterbatch carrier and the butene copolymer reduces bubble stability, raising gauge variability above ±10% on lines without internal bubble cooling and forcing lower screw speed. Terminal articles are 150–200 µm silage bale wrap, 180–250 µm greenhouse cladding, low tunnel covers, and black/white mulch films. Outdoor property retention is tracked by tensile energy at break per ISO 527-3 after xenon-arc exposure per ISO 4892-2; this grade is selected for the base layer, not as the only UV-protected skin, because butene copolymers exhibit lower intrinsic puncture retention after weathering than higher-alpha-olefin grades at equal stabilizer loading.
For cast stretch film lines equipped with 30:1 L/D barrier screws and three-layer feedblocks, Flexirene FG 20 U is positioned as a core-layer economic modifier at 20–50 wt% of total film weight, combined with 40–60 wt% metallocene octene LLDPE and 5–10 wt% LDPE. Skin layers are formulated with 1.5–4.0 wt% tackifier masterbatch, typically polyisobutylene or specialty ester, to achieve cling values measured by ASTM D5458; the butene copolymer core is not used for cling because its surface tack retention falls below specification after 7–14 days of roll storage. Industrial pallet wrap compliance is under EC No 1907/2006; food-contact end uses are not claimed without migration testing under EU 10/2011. The cast line runs at melt temperature 240–260 °C, chill roll temperature 15–25 °C, and gauge 12–25 µm; line speed is typically 300–600 m/min, and edge trim is recycled into the core layer at up to 10 wt% provided gel formation is controlled by fine screen packs. Terminal products are hand stretch wrap and machine pallet wrap. The critical operational boundary is puncture and tear retention under pre-stretch: at FG 20 U content above 50 wt%, puncture propagation resistance measured by ASTM D5748 and Elmendorf tear by ASTM D1922 decline relative to metallocene-rich films; published data for this exact FG 20 U blend ratio is limited, so converters validate roll performance at 80% stretch on their own pallet-wrapping equipment before standardizing the formulation.
| Downstream sector | Compliance and test standards | Typical formulation range | Terminal article type |
|---|---|---|---|
| Heavy-duty liners and shipping sacks | REACH (EC) No 1907/2006; ISO 6383-2; ASTM D1709-A | FG 20 U 75–90 wt%; LDPE 10–20 wt%; carbon black masterbatch 2.5–5.0 wt% | 100–200 µm sacks; 80–150 µm liners |
| Food-contact sealant webs | EU 10/2011 Annex I; FDA 21 CFR 177.1520; ASTM F88 | FG 20 U 65–85 wt%; LDPE 10–25 wt%; plastomer 5–15 wt% | 25–70 µm food pouches; bag-in-box liners |
| Agricultural silage and greenhouse film | EN 13206:2017; ISO 527-3; ISO 4892-2 | FG 20 U 80–95 wt%; LDPE 5–15 wt%; HALS/UV masterbatch 5–8 wt% | 150–200 µm silage wrap; 180–250 µm greenhouse cladding |
| Cast stretch wrap | REACH; ASTM D5458; ASTM D5748 | FG 20 U 20–50 wt%; metallocene LLDPE 40–60 wt%; tackifier 1.5–4.0 wt% | 12–25 µm hand and machine wrap |
| General-purpose household liners | REACH; ASTM D1894; ASTM D1709-A | FG 20 U 70–90 wt%; LDPE 10–20 wt%; slip/antiblock masterbatch 2–4 wt% | 15–40 µm household liners; carrier bags |
| Breathable hygiene backsheet | REACH; ISO 15106-1 | FG 20 U 35–45 wt%; CaCO3 50–60 wt%; TiO2/LDPE masterbatch 5–10 wt% | 25–40 g/m² diaper and incontinence backsheets |
Household liner and carrier bag conversion selects this butene copolymer at 70–90 wt% with 10–20 wt% LDPE, 2–4 wt% combined slip/antiblock masterbatch, and, for dark refuse sacks, 2–5 wt% carbon black masterbatch. Compliance is limited to REACH and local packaging waste requirements; direct food contact is not intended. Processing on high-output blown film lines with internal bubble cooling, die gap 1.8–2.2 mm, and BUR 3.0:1–3.5:1 is performed at melt temperature 180–210 °C; capacitive thickness sensors and segmented die control hold gauge at 15–40 µm across web widths up to 1,600 mm. The slip/antiblock masterbatch is selected to produce a surface coefficient of friction of 0.15–0.25 measured by ASTM D1894 after 48 h maturation, preventing roll blocking without excessive printability loss. Terminal articles are household waste liners, bin liners, retail carrier bags, and drawstring refuse sacks. The operational boundary is melt fracture: at melt temperature below 175 °C or die gap below 1.6 mm, sharkskin roughness appears on the bubble surface and reduces dart impact under ASTM D1709-A; the condition is corrected by raising die temperature or widening die gap rather than by increasing screw speed.
In breathable hygiene backsheet film lines using highly filled CaCO3 formulations, Flexirene FG 20 U is incorporated into the polyolefin matrix at 35–45 wt% together with 50–60 wt% surface-coated calcium carbonate and 5–10 wt% TiO2/LDPE masterbatch; the calcium carbonate is pre-dried to 0.05 wt% maximum moisture and fed through a side-stuffer on a twin-screw compounder with 40:1 L/D. Compliance for hygiene applications follows REACH and product-specific extractables protocols; food-contact regulations are not applicable. The filled film is cast on embossed chill rolls at 15–30 °C and then stretched in machine direction at draw ratios of 2.0:1–4.0:1 to generate microvoids around filler particles; moisture vapour transmission rate is measured by ISO 15106-1 after lamination, and the process window is narrow because excess draw ratio above 4.0:1 tears the web at filler agglomerates while draw ratio below 2.0:1 leaves breathability below specification. Terminal articles include breathable backsheets for infant diapers, adult incontinence products, and feminine hygiene pads in basis weights from 25 g/m² to 40 g/m². Published data for FG 20 U in this exact filled system is limited; converters therefore validate filler dispersion and draw-ratio windows on pilot-scale cast film equipment before committing to production-scale runs.
Competitive Versalis Flexirene® FG 20 U Butene Copolymer Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Versalis Flexirene® FG 20 U is a butene-1 copolymer linear low-density polyethylene supplied as free-flowing pellets for blown film extrusion. In the lot-certificate data, the two primary specification anchors are a nominal melt flow rate of 2.0 g/10 min measured at 190 °C under 2.16 kg load in accordance with ISO 1133-1:2022, and a nominal density of 0.918 g/cm³ determined by ISO 1183-1:2019. The “U” designation identifies a factory-compounded stabilisation and processing-aid package; it is not equivalent to downstream addition of slip or antiblock masterbatches.
Within the Versalis polyethylene range, the grade is positioned for general-purpose blown film rather than cast film, extrusion coating, or injection moulding. Its melt flow rate of 2.0 g/10 min places it between fractional-MFI heavy-sack film grades and high-flow injection-moulding grades, balancing die pressure and draw-down. The resin is polymerised with butene-1 as the α-olefin comonomer, so the short-chain branch distribution differs from hexene-1 and octene-1 copolymers. That difference in branch length and placement has direct consequences for film toughness, tear resistance, seal response, and processing behaviour.
In solid-state deformation, the butene-1 branch is shorter than the hexene-1 or octene-1 branch and generates a less efficient tie-molecule network between adjacent lamellae at equal density. The practical outcome is that a butene-based LLDPE typically exhibits lower Elmendorf tear and dart drop values at the same film gauge. For Flexirene® FG 20 U, converter-reported 40 µm films commonly show a dart impact F50 of 100 g to 120 g under ASTM D1709-16a Method A, and Elmendorf tear values near 110 N/mm machine direction and 250 N/mm transverse direction under ISO 6383-2:1983. These values are sufficient for general-purpose bags, sleeve wrap, and stretch film but are not positioned for high-dart industrial liners or heavy-gauge agricultural film. The lower density and reduced crystalline fraction also lower the heat-seal initiation temperature; this behaviour can reduce jaw set-point requirements in vertical form-fill-seal equipment, although seal strength should be measured on the finished structure under ISO 527-3:2018 or equivalent.
The low density of 0.918 g/cm³ places FG 20 U in the lower-density segment of the LLDPE range. This reduces secant modulus and tensile yield stress while increasing elongation and impact toughness relative to a butene LLDPE at 0.924 g/cm³. The density value is determined on compression-moulded specimens, whereas blown film properties depend on cooling rate, orientation, frost-line height, and film thickness. Table 1 lists nominal values frequently reported for a 40 µm blown film produced on a smooth-bore extruder with a 30:1 L/D and a die gap of 1.2 mm. These are typical characterisation values, not lot-release specification limits, and they should be verified against the certificate of analysis for the specific lot.
| Property | Test method | Unit | Nominal value |
|---|---|---|---|
| Melt flow rate | ISO 1133-1:2022 | g/10 min | 2.0 |
| Density | ISO 1183-1:2019 | g/cm³ | 0.918 |
| Dart impact F50 | ASTM D1709-16a Method A | g | 100–120 |
| Elmendorf tear MD/TD | ISO 6383-2:1983 | N/mm | 110 / 250 |
| Tensile stress at yield MD/TD | ISO 527-3:2018 | MPa | 11 / 10 |
| Elongation at break MD/TD | ISO 527-3:2018 | % | 700 / 800 |
| Haze | ISO 14782:1999 | % | 8 |
| Gloss 60° | ASTM D2457-19 | dimensionless | 80 |
| Melting temperature | ISO 11357-3:2018 | °C | 122 |
| Vicat softening point A/50 | ISO 306:2022 | °C | 95 |
On a production-scale blown film line equipped with a 75 mm or 90 mm grooved-feed extruder, a barrier screw with a Maddock shear mixer, and a dual-lip air ring, the grade is generally processed with melt temperatures from 190 °C to 230 °C. Higher melt temperatures may increase bubble instability because the resin lacks the long-chain branching needed to resist extensional thinning. The recommended die gap is between 1.0 mm and 2.5 mm; wider gaps reduce gel sensitivity but may increase haze because internal melt shear is lower. Typical blow-up ratios lie between 2.0:1 and 3.0:1, and frost-line heights are set from 4 to 8 die diameters depending on the desired balance of dart and tear. When processing on a high-stalk configuration, internal bubble cooling is strongly advised; without it, backside cooling is insufficient and gauge fluctuation may exceed ±5% on thin-gauge widths above 1,200 mm.
The screw design should include a barrier section and a Maddock mixer because the grade, like other LLDPE, has a narrower melting range and higher melting torque than LDPE. A grooved-feed extruder is preferred for stable transport; smooth-bore extruders can be used if throughput is reduced. The screen pack should be changed when head pressure rises by more than 15% over the clean start-up value, because pressure build-up is an early indicator of gel accumulation or degradation. At die gaps above 2.5 mm, the melt may not be sufficiently sheared to eliminate some gel defects, while die gaps below 1.0 mm can create excessive head pressure and melt fracture on conventional lines.
In coextruded structures, FG 20 U is often assigned to the core or the outer skin where its low gel count and stable viscosity in the shear-rate range of 100 s⁻¹ to 1,000 s⁻¹ allow consistent thickness distribution. Because melt strength is limited, the grade should not be used as the sole polymer in high-stalk tubular film lines that require a long bubble neck unless an air-ring upgrade and internal bubble cooling are installed. Regrind levels must be validated for the specific film structure; contamination by polypropylene, paper fibre, or ethylene-vinyl acetate residues produces dimensional instability and optical defects. For printing and metallisation, external slip additives in coextruded skins must be re-evaluated because they can reduce surface energy and ink adhesion.
The melt rheology of FG 20 U is characteristic of a linear butene α-olefin copolymer. Shear viscosity at 190 °C is lower than that of a branched LDPE at high shear rates, but extensional viscosity is lower at all strain rates. This explains why the bubble is less resistant to draw resonance in high-stalk film lines. The use of a melt pump is recommended for automatic packaging applications because it can reduce output variation to below ±1% and stabilise the frost line. On extruders without a melt pump, screw-speed variation is transmitted directly to film thickness and may create bands of low dart impact in the final roll.
The most significant differentiator between Flexirene® FG 20 U and a higher α-olefin LLDPE is lower dart impact and tear retention at equal density and melt index. At a density of 0.918 g/cm³ and a melt flow rate of 2.0 g/10 min, a hexene-1 or octene-1 grade generally develops a higher tie-molecule fraction during blown film orientation. The butene-based grade compensates with lower comonomer cost and easier melt homogenisation on extruders with limited mixing capacity. Its lower melting point and broader melting curve can also permit lower seal-bar temperatures than a medium-density or high-density polyethylene. However, converters attempting to down-gauge below 25 µm should closely monitor dart impact and puncture resistance; published data for this specific configuration is limited, so pilot-line trials with the actual die geometry and cooling setup are required before commercial commitments.
Compared with metallocene-catalysed hexene LLDPE, the broader molecular weight distribution of FG 20 U may generate a wider heat-seal plateau but slightly lower hot-tack strength. The butene-1 comonomer reduces the number of high-strength tie chains, which is detected as lower puncture resistance and lower slow crack growth resistance under constant load. These differences are most visible in films stretched above 200% during pallet wrapping or in heavy-gauge liners subject to sharp protruding loads. For those applications, a converter may select a higher α-olefin grade or a coextruded structure with an outer octene-based layer.
In contrast to autoclave or tubular LDPE, FG 20 U has no long-chain branching. The practical consequences are lower die swell, lower melt tension, and a less shear-thinning viscosity curve in the shear-rate range typical of extrusion dies. When replacing LDPE in an existing line, the die gap may need to be reduced and the melt temperature lowered by 5 °C to 10 °C to preserve bubble geometry. Dart impact and tensile strength are generally improved relative to LDPE at the same gauge, which permits down-gauging from 60 µm to 40 µm in some bag applications. The improvement is not uniform across all film properties, and tear balance must be checked in the machine and transverse directions.
Primary converting applications for Flexirene® FG 20 U include general-purpose blown films in the gauge range 20 µm to 120 µm, such as garment bags, produce bags, magazine overwrap, and hand- or machine-wrap stretch film. The grade is not optimized for high-dart trunk liners or heavy-gauge industrial liners where octene-based LLDPE is preferred. In coextruded structures, it is commonly placed in a core or skin layer where its melt pump stability is acceptable. For primary food packaging, migration testing should be performed on the finished article under the intended time and temperature conditions rather than inferred only from resin compliance.
Regulatory qualification depends on the finished article and converting conditions, not only on the resin. The manufacturer-supplied declarations for Flexirene® FG 20 U generally place the grade within the scope of the following frameworks when the film is produced at melt temperatures below 240 °C and without prohibited additives.
| Framework | Condition or limit |
|---|---|
| EU Plastics Regulation (EU) No 10/2011 as amended | Overall migration limit 10 mg/dm²; final-article testing under intended food simulant and time/temperature conditions is required |
| FDA 21 CFR 177.1520(c) 3.2 | Olefin polymers for food contact; end-use limitations and migration testing apply to the finished article |
| REACH (EC) No 1907/2006 Article 33 | Substances of very high concern below 0.1% w/w in the article; verify against safety data sheet and supplier declaration |
| RoHS Directive 2011/65/EU | For electrical and electronic equipment housings: Pb 0.1%, Hg 0.1%, Cd 0.01%, Cr(VI) 0.1%, PBB 0.1%, PBDE 0.1% by weight in homogeneous material |
Storage of resin in a clean, dry area below 30 °C is standard. Drying is not normally required, but if the pellets have been exposed to relative humidity above 60% for extended periods, surface moisture can generate surface roughness and streaks on the film. A dehumidifying hopper dryer operating at 70 °C for 2 h can restore processing consistency. The grade should not be processed at melt temperatures above 240 °C, because degradation of the stabiliser package and formation of gel particles increase with residence time. Equipment purging after processing PVC, PVDC, or acetal resins is required because chlorine or aldehyde residues can cause polymer decomposition and die-lip build-up.