| HS Code | 446726 |
| Polymertype | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | 1-Octene |
| Density | 0.923 g/cm³ |
| Meltflowrate 190c 2 16kg | 0.8 g/10 min |
| Meltflowratio 21 6 2 16 | 27 |
| Tensilestrengthatyield | 11 MPa |
| Tensilestrengthatbreak | 30 MPa |
| Elongationatbreak | 700% |
| Flexuralmodulus | 260 MPa |
| Vicatsofteningtemperature | 100 °C |
| Meltingtemperature | 122 °C |
| Dartdropimpact | 250 g |
| Elmendorftearstrength Md | 200 g |
| Elmendorftearstrength Td | 400 g |
| Haze | 12% |
| Gloss 45deg | 60% |
| Coefficientoffriction | 0.2 |
| Blocking | 30 g |
As an accredited Versalis Clearflex® H&T LFH 238 Octene Copolymer Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Versalis Clearflex® H&T LFH 238 is supplied in 25 kg polyethylene bags, 40 bags per 1,000 kg stretch-wrapped pallet for industrial handling. |
| Container Loading (20′ FCL) | Palletized 25kg bags of Versalis Clearflex® H&T LFH 238 octene copolymer LLDPE, approx. 18–20 MT net, loaded in dry 20′ FCL. |
| Shipping | Versalis Clearflex® H&T LFH 238 Octene Copolymer Linear Low Density Polyethylene is shipped as solid pellets in 25 kg bags or 1,000 kg bulk bags, palletized and stretch-wrapped. Transport by truck, rail, or container at ambient temperature. Keep dry, clean, away from moisture and sunlight. Non-hazardous; follow SDS and local rules. |
| Storage | Store Versalis Clearflex® H&T LFH 238 in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, sparks, and flames. Keep original packaging sealed and protect from moisture, dust, and contamination. Avoid strong oxidizers. Maintain ambient temperature, stack securely to prevent bag rupture, and follow local regulations. Use grounding and static control when handling bulk. Do not store outdoors. |
| Shelf Life | Typically 24 months when stored in original, unopened packaging under cool, dry, shaded conditions, away from direct sunlight and heat. |
On a three-layer blown-film line running 50–55 µm frozen vegetable packages at 180–220 kg/h, Clearflex H&T LFH 238, an octene-copolymer linear low density polyethylene, is typically placed in the core and sealant layers to preserve low-temperature dart resistance and seal integrity through freezing tunnels. The extruder set-up consists of a 75 mm barrier screw with L/D 30:1 and a Maddock mixing section, a 250 mm annular die, and a die gap of 1.8 mm; melt temperature is held at 195–210°C, and the bubble is drawn at a blow-up ratio of 2.8:1 with frost line height at 7 die diameters. Converter validation involves falling-dart impact at −20°C according to ASTM D1709-16, method A, because frozen food packaging is handled at sub-zero temperatures after filling and sealing. Heat-seal strength is measured by ASTM F88-21 on 25.4 mm wide strips after sealing at 130°C, 0.5 MPa jaw pressure, and 1.0 s dwell. Food-contact compliance relies on FDA 21 CFR 177.1520(c) 3.2a for ethylene/1-octene copolymers and on EU No 10/2011 overall migration below 10 mg/dm² using food-appropriate simulants. The melt temperature ceiling is 230°C; above this threshold gel formation and organoleptic deviation increase. Regrind loading is limited to 20 wt% in the core layer only, while post-industrial film with surface treatment or slip agents is not recycled into the sealant layer above 10 wt% due to hot-tack suppression. No resin pre-drying is required below 60% RH; if external storage under humid conditions has caused surface condensation, a 60°C hopper dryer for 2 h removes surface moisture without pre-melting pellets. Surface treatment to 38 dyn/cm is omitted for direct frozen food packs, but if printing or lamination follows, inline corona at 2.2 kW is applied after the nip rolls.
In stretch hood conversion for palletized building products or beverages, Clearflex H&T LFH 238 is processed as a three-layer blown film with total thickness between 140 µm and 180 µm and a target hood deformation of 50–60% during application. The line configuration includes a 400 mm die, 2.2 mm die gap, and melt temperature from 190°C to 205°C; output ranges from 320 kg/h to 380 kg/h depending on downstream collapsing and winding. The critical mechanical property is not only dart impact at ambient temperature but stress retention after sustained elongation, measured by ASTM D5459 at 250 mm/min crosshead speed and a pre-stretch ratio of 100–200%; converters commonly impose a permanent deformation below 12% and a force retention above 40% at 30 s after stretch, although published data for this specific configuration is limited and must be confirmed with production lots. At −18°C, pallet stability depends on low-temperature puncture resistance under film tension; ASTM D5748 is applied with a 75 mm probe to detect micro-pinholes initiated at corner folds. Heat-seal or adhesive-free overlap is used, so edge tear resistance measured by ASTM D1922 in both machine and transverse directions becomes a gate criterion; machine-direction tear values below 300 g per 25 µm of film typically correlate with hood splitting at bottom pallet edges. The processing window for LFH 238 in this application is limited by bubble stability at high blow-up ratios; die pressure should remain below 35 MPa, and internal bubble cooling is required to prevent frost-line oscillation above 8 die diameters.
When a 1200 mm cast-film die is operated with LFH 238 in the cling layer of a 25 µm silage bale wrap, the concentrate feed includes 2–3 wt% polyisobutylene, a 0.2–0.5 wt% hindered amine light stabilizer package, and, for white-opaque grades, 4–6 wt% rutile titanium dioxide predispersed in LLDPE carrier. The cast line uses a 0.5 mm die gap, a chill roll set point of 20°C, and line speed sufficient to produce 400–450 kg/h; edge trim from the 1200 mm die is reground into the core at 5–10 wt%. Migration of polyisobutylene to the film surface reaches steady state within 24–48 h; coefficient of friction during this period shifts from approximately 0.70 to 0.30 when tested by ISO 8295, which influences reel slitting and on-farm unwinding. Tensile properties are measured by ISO 527-3 on 15 mm wide specimens at 500 mm/min, and puncture impact is tested with ISO 7765-2 using a 38 mm hemispherical striker at 23°C; UV durability is usually assessed by ISO 4892-2 for 300–500 h before measurable tensile loss occurs, but the additive masterbatch type and film thickness determine actual field life. The main operational boundary is printability: high polyisobutylene migration makes the cling surface unsuitable for corona treatment and ink adhesion below 38 dyn/cm; if printed identification is required, a non-cling outer layer must be incorporated or the cling additive level reduced below 1.5 wt%. Storage of finished reels above 35°C accelerates polyisobutylene migration and can cause blocking at the core, especially when winder tension exceeds 12 N/mm.
Sack drop testing, rather than film tensile data alone, drives the formulation for 25 kg and 50 kg heavy-duty sacks made with a three-layer tubular blown film containing LFH 238 in the inner sealing layer. The die is 300 mm in diameter with a 1.6 mm gap; melt temperature is held at 200–215°C, blow-up ratio at 2.4:1, and frost line height at 5–6 die diameters. A representative structure is outer HDPE of 15 µm, core recycled LLDPE/LDPE of 35–40 µm, and inner LFH 238 of 20–25 µm, producing total film thickness of 70–80 µm. Qualification uses ISO 7965-2 sack drop tests with a 25 kg filled sack at 1.2–1.5 m drop height, with conditioning at 23°C and −10°C; a passing lot typically shows no sealing seam burst and no side-wall penetration after three drops, though published data for this specific configuration is limited and must be confirmed in production trials. The octene copolymer architecture provides higher tear propagation resistance than butene-copolymer LLDPE at equivalent density, but the tensile modulus measured by ISO 527-3 decreases by approximately 10–15% when compared with a butene grade of similar melt flow, which requires the outer HDPE layer to compensate bending stiffness. Side-wall abrasion is evaluated according to ISO 1518; sacks that fail this test exhibit localized thinning at the contact point and subsequent tear propagation during repeated pallet shifting. The inner layer heat seal is made at 135–150°C with 0.5 s dwell and 0.4 MPa pressure, and hot tack is measured by ASTM F1921 immediately after seal opening at 50 mm/s. Process boundaries include die build-up if the core layer contains recycled material with gel particles above 200 µm, so a 100 mesh screen pack is required in the core extruder.
Blown film for barrier laminates is produced from LFH 238 at 40 µm thickness and then corona-treated to 38–40 dyn/cm before lamination against aluminium or metallised polyester with a solventless polyurethane adhesive applied at 2.0 g/m². Heat-seal initiation of the octene-copolymer sealant web is typically observed at 95–105°C with a plateau from 120°C to 140°C; peel strength is measured according to ASTM F88-21 on 25.4 mm wide strips using 0.275 MPa jaw pressure, 1.0 s dwell, and 200 mm/min peel rate. The sealant layer must comply with the following checklist before conversion for dry powders or liquid condiment sachets:
| Regulation/Standard | Clause or Test Designation | Acceptance Criterion |
|---|---|---|
| FDA 21 CFR 177.1520(c) 3.2a | Ethylene/1-octene copolymer food-contact | Conditions of use A through H per 21 CFR 176.170(c) |
| EU No 10/2011 | Overall migration | < 10 mg/dm² in food-appropriate simulants |
| REACH Article 33 | SVHC communication | < 0.1% w/w |
| 94/62/EC | Packaging heavy metals | Sum of Pb, Cd, Hg, Cr VI < 100 mg/kg |
The operational boundary for this sealant web is retort and hot-fill handling: the film should not be specified for retort cycles above 110°C because LLDPE crystals begin to melt around 120–125°C, and bag deformation under internal pressure can occur at 121°C saturated steam. If a converter requires retortable pouches at 121°C, a polypropylene-based sealant is substituted, or the laminate is reformulated with a thicker outer polyester layer to restrain creep. For non-retort packaging, extractable studies must be performed on the complete laminate because the adhesive and print layers also contribute to migration, and the LFH 238 sealant web cannot be considered automatically compliant without testing the final article under EU No 10/2011.
High-draw cast pallet wrap is converted from LFH 238 on a single-screw cast line with a 150 mm screw, L/D 30:1, a 2600 mm flat die, and a 0.5 mm die gap; melt temperature at the die lip is maintained between 220°C and 235°C. Output for a 10–12 µm final film typically reaches 600–650 kg/h, with chill roll setpoints at 20°C and 25°C and line speed above 500 m/min. Pre-stretch at the wrapping machine is set between 250% and 300%; at this level, melt must resist neck-in during casting, which is typically held below 12% of die width by adjusting melt pooling and draw ratio. Force retention after stretching is measured by ASTM D5459 at 200% elongation and 30 s relaxation; films with inadequate octene comonomer distribution show rapid loss of load-holding force and excessive permanent deformation above 15%. Puncture resistance is measured by ASTM D5748, while on-pallet load containment is validated by ASTM D4169-22 truck profile or the EUMOS 40509 stability method; published data for this specific configuration is limited, and converter qualification generally requires a side-by-side run against an incumbent resin at the same pre-stretch ratio. Cling is imparted by polyisobutylene at 2–4 wt% in the outer skin; blocking becomes a risk when reel storage exceeds 30°C or when winder tension exceeds 14 N/mm. A synthetic silica antiblock at 500–1500 ppm is sometimes included in the opposite skin to control roll unwinding without excessively reducing film clarity.
Competitive Versalis Clearflex® H&T LFH 238 Octene Copolymer Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Versalis Clearflex H&T LFH 238 is an octene-1 comonomer linear low density polyethylene supplied for blown and cast film conversion. The grade identification specifies an ethylene/1-octene copolymer with short-chain branches distributed along the polyethylene backbone. The octene-derived branch is longer than the branch introduced by butene-1 or hexene-1, which alters the distribution of crystallisable sequences and tie-molecule formation. Density and melt mass-flow rate for LFH 238 are measured according to ISO 1183-1 and ISO 1133-1:2022, respectively; the current supplier technical data sheet should be used for specification verification because commercial lot-to-lot variation may occur within the certified range. Food-contact suitability for the base olefin polymer may be assessed under FDA 21 CFR 177.1520 and EU Regulation (EC) No 1935/2004, provided that the specific additive package meets applicable migration limits.
The H&T designation is associated with high tenacity and puncture-oriented film performance, but process selection should not rest on the family descriptor alone. In contrast to high-pressure low density polyethylene, the LFH 238 grade does not contain the same long-chain branching distribution; consequently, its melt extension behaviour at the bubble and its shear thinning response differ. In cast and blown film production, these differences appear as changes in neck-in, bubble stability, and orientation-induced mechanical response. Published data for LFH 238-specific configurations is limited; comparative trial production on the target line is therefore required to establish an output-to-toughness relation for a given die and haul-off configuration.
The product is an octene-copolymer LLDPE, meaning the comonomer content is adjusted to obtain density values typically between 0.915 g/cm³ and 0.925 g/cm³ for film grades when tested by ISO 1183-1. Melt flow rates for film resins of this family commonly fall between 0.5 g/10 min and 2.0 g/10 min at 190 °C with 2.16 kg load. Exact LFH 238 values are not restated here because they may change with production site and grade revision.
Comonomer type influences the length of the short-chain branches excluded from the polyethylene crystal lattice. Butene-1 introduces shorter branches, hexene-1 introduces intermediate branches, and octene-1 introduces longer branches. Because the branch length increases, the probability that a branch will be rejected from a lamella increases, and the number of interlamellar tie molecules can rise. The effect is evaluated by dart impact tests using ASTM D1709 or ISO 7765-1, Elmendorf tear using ASTM D1922 or ISO 6383-2, and tensile energy-to-break using ISO 527-3.
| Comonomer | Branch character | Dart impact resistance | Elmendorf tear resistance | Haze tendency | Seal initiation tendency |
|---|---|---|---|---|---|
| Butene-1 | Short | Lower | Lower | Higher | Higher |
| Hexene-1 | Intermediate | Intermediate | Intermediate | Intermediate | Intermediate |
| Octene-1 | Longer | Higher | Higher | Lower | Lower |
At film thickness below 50 µm, impact failure is often governed by crack propagation and lamellar orientation rather than gross yielding. Octene-copolymer LLDPEs of this class usually retain higher dart impact resistance and tear resistance at an equivalent density than butene-based LLDPEs, although gauge control and frost-line temperature can obscure these differences on a production line. For LFH 238, the quoted balance of dart, tear, and optics should be checked on the specific film tower because nip-induced orientation and heat transfer differ between spiral mandrel dies, radial distributor dies, and flat cast dies. In a cast film line, chill-roll temperature below the crystallisation onset can freeze surface nuclei and reduce film clarity; in a blown film line, a lower frost line height may increase film crystallinity and reduce impact performance.
Agricultural greenhouse and silage stretch film applications subject the material to long-term axial tension and ultraviolet oxidative attack. The base octene LLDPE does not provide intrinsic UV stability; hindered amine light stabilizers and phenolic antioxidants are introduced by masterbatch or compounding. Required weathering performance is typically verified by accelerated xenon-arc exposure according to ISO 4892-2 and subsequent tensile retention per ISO 527-3. For LFH 238, product selection should include oxidative induction time data obtained by ISO 11357-6 and retained tear strength after exposure. Published data for LFH 238-specific weathering configurations is limited; field failures in exposed films commonly appear as brittle cracking at fold creases and edge-slit tear propagation rather than uniform elongation loss. Stabilizer efficiency can be reduced by contact with acidic pesticide residues or by storage near transition metal ions such as iron and copper.
Extrusion of octene LLDPE on blown film lines requires attention to die gap, melt temperature, and bubble cooling. Narrow die gaps below 1.2 mm can produce high shear stress at the lip and may trigger surface melt fracture if the melt temperature remains below 190 °C. Wider die gaps of 2.0–2.4 mm reduce die pressure but may lower melt orientation and degrade film optics. Typical blown film extruders for this resin class use 24:1 to 30:1 L/D ratios, medium compression screws, and spiral mandrel distributor dies. Internal bubble cooling can raise output by 20–40 % relative to single-lip air ring cooling in general-purpose LLDPE lines, but the higher frost line height may reduce film modulus if the quench is too delayed.
On production lines, a batch-to-batch melt flow rate shift of 0.1 g/10 min at the specification boundary can move the frost line and alter bubble stability; operators may compensate with 5–10 °C temperature adjustments or haul-off speed changes. For LFH 238, real-time monitoring of die pressure, motor load, and bubble diameter is recommended because published data for this specific configuration is limited. Surface melt fracture, bubble sag, and gauge bands are the dominant failure modes when the processing window is exceeded. The frost line should not be allowed to drop below 3 die diameters when stable bubble geometry is required for gauge uniformity.
In coextruded barrier laminates, octene LLDPE is used more often as a sealant skin than as the structural core because its melt strength is lower than high-pressure LDPE and neck-in may be higher in extrusion coating. Seal initiation temperature is a primary process variable in horizontal and vertical form-fill-seal operations. Seal strength is measured according to ASTM F88 or ISO 527-3 on heat-sealed specimens; seal initiation curves are generated at fixed dwell times and pressures. The octene-derived branching in LFH 238 can reduce seal initiation relative to a butene-based LLDPE of equal density, because a lower crystalline melting onset permits molecular interdiffusion at lower jaw temperatures. A seal initiation reduction of 3–5 °C can raise vertical form-fill-seal output by 5–10 % when the line is sealing-limited. Published data for LFH 238-specific sealing curves is limited; the supplier's technical data should be used to set platen temperature because seal strength can plateau after full fusion above approximately 140 °C.
Reformulation from butene-based LLDPE to octene-based LFH 238 in heavy-duty sack film often requires adjustment to the extruder temperature profile and frost line. The melt stiffness below the melting point changes, affecting bubble geometry and collapsing frame friction. Dart impact and tear values should be compared at equal film gauge using ASTM D1709 and ASTM D1922. Tensile properties are assessed by ISO 527-3, and puncture resistance may be evaluated by ASTM D5748 if cling and puncture retention are critical. Differences in melt flow ratio can alter bubble stability, so blending with high-pressure LDPE at 10–20 % may be required for stable pocket formation. This blending, however, reduces toughness; therefore, octene LLDPE is often run at a lower LDPE fraction than butene LLDPE to maintain dart impact performance. The substitution should be validated at the same thickness, frost line height, and collapsing frame pressure because laboratory film-to-film comparisons may not reproduce line-specific orientation effects.
Blown film haze in octene LLDPE is controlled by surface roughness, crystallinity, and additive dispersion. Haze is measured by ASTM D1003 or ISO 14782; gloss is measured by ASTM D2457 at 45 ° incidence. At high throughput, melt temperature may rise beyond the capability of the external air ring, delaying crystallisation and producing larger crystalline domains that scatter more light. For LFH 238, incremental output without additional cooling may raise haze from below 10 % to above 15 % in high-clarity film structures. Bubble instability below a frost line of 3 die diameters may create chatter bands and thickness variation. A minimum frost line height of 6–8 die diameters is commonly maintained for stable bubble geometry. Published data for LFH 238-specific haze-to-output curves is limited; line trials should measure haze, gloss, and dart impact at 3 output settings to establish the process boundary.
Polyethylene recycling streams accept unfilled octene LLDPE film if density remains below 0.925 g/cm³, as sorting processes separate denser materials. The LFH 238 grade should be considered compatible with standard mechanical recycling under ISO 15270. In practice, high-clarity film lines may blend reprocessed trims up to 15–20 % without measurable loss in dart impact, provided filtration removes gel and char contaminants. The coefficient of friction should be measured according to ISO 8295 when slip and antiblock additive concentrations are changed through reclaimed material addition. Compared with butene-based LLDPE and high-pressure LDPE blends, the difference of LFH 238 lies in its capacity to maintain toughness at reduced gauge while retaining a lower seal initiation tendency. Users should nevertheless verify that internal recycle streams and additive concentrations do not shift the coefficient of friction beyond the range specified for the downstream packaging machine.