| HS Code | 873483 |
| Density | 0.921 g/cm³ |
| Meltflowrate 190c 2 16kg | 0.9 g/10 min |
| Meltingpoint | 124 °C |
| Vicatsofteningtemperature 10n | 96 °C |
| Tensilestrengthatbreak Md | 35 MPa |
| Tensilestrengthatbreak Td | 30 MPa |
| Elongationatbreak Md | 600 % |
| Elongationatbreak Td | 700 % |
| Secantmodulus 1 Md | 210 MPa |
| Secantmodulus 1 Td | 230 MPa |
| Dartdropimpact F50 | 120 g |
| Elmendorftearresistance Md | 120 g |
| Elmendorftearresistance Td | 250 g |
| Haze | 12 % |
| Gloss 45 Degrees | 60 % |
As an accredited Versalis Clearflex® FG 306 A Film Grade LLDPE factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg PE bags, 40 bags per shrink-wrapped 1,000 kg pallet, supplied in truckload quantities for industrial use. |
| Container Loading (20′ FCL) | Versalis Clearflex® FG 306 A Film Grade LLDPE: 20′ FCL loads 25 kg palletized bags, shrink-wrapped, approximately 20 MT net. |
| Shipping | Versalis Clearflex® FG 306 A Film Grade LLDPE is shipped as non-hazardous, free-flowing pellets in 25 kg polyethylene bags or octabins, palletized and stretch-wrapped. Transport in clean, dry trucks or containers at ambient temperature, avoiding moisture, direct sunlight, excessive heat, and ignition sources. |
| Storage | Store Versalis Clearflex® FG 306 A Film Grade LLDPE in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, sparks, and flames. Keep original bags sealed on pallets to prevent moisture, dust, UV degradation, and contamination. Avoid strong oxidizers. Maintain stable stacking and good housekeeping. Use FIFO stock rotation. Refer to supplier SDS for detailed storage requirements. |
| Shelf Life | Shelf life: two years when stored unopened in original packaging, dry, cool conditions, away from direct sunlight and heat. |
In silage wrap production, FG 306 A is typically run as a monolayer or three-layer film of 25 µm nominal thickness, with a compounded density of 0.920 g/cm³ after addition of a 10–12 wt% HALS/UV masterbatch. The masterbatch uses a polymeric hindered amine with molecular weight above 1,000 g/mol and a triazine UV absorber at a total active content of 8–10%. The processing window is narrow because the low-molecular-weight carrier in the masterbatch lowers melt viscosity; feed throat temperature above 45°C on a 75 mm barrier screw induces screw slippage and throughput variation. Throughput on the same line at 70 rpm is typically 140–160 kg/h, and output fluctuation beyond ±5% indicates feed throat bridging or masterbatch carrier segregation. Melt temperature at the die is held below 240°C and residence time below 5 min to limit thermal decomposition of the hindered amine. Blow-up ratio is set at 2.2:1 to 2.8:1 and frost line height at 600–800 mm above the die. At lower frost line heights, UV stabiliser migration to the film surface increases initial tack but causes tack/slip drift after 120 days of outdoor storage; the coefficient of friction shifts from 0.30 to 0.55 when measured by ISO 8295:1995. The terminal product is stretched over silage bales, requiring sustained elongation of 60–80% to exclude oxygen from the ensiled forage. Elmendorf tear in the machine direction, measured by ISO 6383-2:1983, should remain above 120 g to prevent tearing on rotating-arm wrappers.
Dart impact by ISO 7765-1:1988 is controlled through die gap and frost line height. A die gap of 1.8–2.4 mm promotes transverse orientation that raises TD tear while reducing MD tear; therefore the converter must avoid die gaps below 1.8 mm for silage wrap unless the bubble is intentionally stabilized with internal bubble cooling. When UV masterbatch loading exceeds 12 wt%, die lip plate-out of oligomeric carrier components occurs after 4–6 h on standard chrome dies; ceramic-coated die lips extend the run to 8 h before cleaning is required. The final roll must be protected from edge exposure to sunlight because uneven UV absorber consumption produces brittle bands at the roll shoulders. Published data for the specific UV retention plateau of FG 306 A in multi-season silage wrap is limited; validation by xenon-arc weathering to ISO 4892-2:2013 with burst strain retention after 1,000 h is required before field use.
At 60 µm and above, blown film lines running FG 306 A for inner ply webs in heavy-duty shipping sacks operate inside a melt fracture boundary that is controlled by die lip shear rate and metal surface condition. The resin is blended with 30–40 wt% LDPE with melt flow rate 0.3 g/10 min and density 0.923 g/cm³ to stabilise bubble dynamics and reduce dart impact variability. The die gap is increased from 1.6 mm to 2.0 mm, and melt temperature is raised to 225°C–235°C. Internal bubble cooling delivers air at 15–20°C and 1,200–1,500 m³/h to hold a frost line height of 400–600 mm at a blow-up ratio of 2.0:1 to 2.5:1. The terminal inner ply is used on form-fill-seal lines for granular chemicals and thermoplastic resin packaging. Dart impact according to ISO 7765-1:1988 is specified at a minimum of 200 g on 60 µm film, while Elmendorf tear by ISO 6383-2:1983 is balanced at 140 g MD and 220 g TD. A drop in TD tear below 180 g after incorporating more than 15 wt% recycled edge trim has been observed on production lines; the correction is to raise the frost line by 100 mm rather than to increase total thickness, because greater frost line height relaxes frozen-in orientation without sacrificing output.
The FG 306 A inner ply is formulated without migratory slip or antiblock if the outer ply will be printed and coated; surface tack control is therefore managed through density adjustment and chill roll temperature. Screw speed on a 75 mm single-screw extruder with a 30 L/D barrier screw and Maddock mixing section is set at 85 rpm, with melt pressure between 280 bar and 320 bar. A screen pack of 20/40/60/80 mesh is installed before the die; pressure increase above 350 bar within 24 h indicates gel accumulation from degraded regrind and requires screen replacement. Aminous processing aids should be excluded from the inner ply because residual amines can impart odour to packaged chemical contents and may interfere with corona treatment of the outer ply. Compliance for the shipping sack construction is assessed under EU Packaging and Packaging Waste Directive 94/62/EC, Annex II, for heavy metals, with total lead, cadmium, mercury and hexavalent chromium not exceeding 100 mg/kg combined.
Frozen food packaging converters specify FG 306 A as the carrier web in solventless lamination of biaxially oriented polyester or biaxially oriented polypropylene to a coextruded sealant film. The sealant web contains a core of FG 306 A at 80–90 wt% and an EVA seal layer with 12–18% vinyl acetate content at 10–20 wt%. The core melt temperature is set at 230°C, while the EVA layer is limited to 205°C to prevent acetic acid generation and odour development. Blow-up ratio is held at 2.0:1 to 2.4:1 and total web thickness at 45–60 µm. Solventless lamination bond strength is measured after 48 h cure by ISO 10364:2015; peel strength below 2.0 N/15 mm after freezing indicates incomplete corona treatment or low-molecular-weight additive bloom from the FG 306 A core. The terminal pouch or lidding web is used for frozen fish and vegetable packaging. Compliance for the polyolefin components is established under FDA 21 CFR 177.1520 and under Regulation (EU) 10/2011, Annex I, with the overall migration limit of 10 mg/dm² surface area. The converter must confirm that the specific FG 306 A certificate covers the intended frozen food application and the chosen food simulants, because migration data for this grade in a frozen lamination is limited; end-use testing to EU 10/2011 Annex III with simulant A at 20°C for 10 days is required.
Die gap selection in this coextrusion is governed by the EVA layer’s viscosity mismatch. At a die gap of 1.8 mm, a 10 wt% EVA skin can flow preferentially at the die walls and reduce the FG 306 A core thickness below setpoint. The correction is to maintain a die gap of 2.0 mm to 2.2 mm and to set the extruder barrel temperature profile for FG 306 A at 180°C feed, 200°C compression, 220°C metering, and 230°C die. Frost line height is kept at 300–450 mm because excessive cooling creates a wide crystalline orientation gradient that reduces seal strength after lamination. The corona treater should achieve a minimum surface energy of 42 dyn/cm on the FG 306 A side before lamination, measured by ISO 8296:2003 test inks; lower values produce skipped adhesive islands and localised delamination when the pouch is folded at freezer temperatures.
| Scenario | Regulatory reference | Performance test standard |
|---|---|---|
| Cast pallet stretch film | EU 94/62/EC Annex II; REACH Art. 33 | ISO 527-3:2018; ISO 7765-1:1988; ASTM D5748-95(2019) |
| Silage wrap | REACH Art. 33; EU 1272/2008 CLP | ISO 6383-2:1983; ISO 8295:1995; ISO 4892-2:2013 |
| Heavy-duty shipping sack inner ply | EU 94/62/EC Annex II | ISO 7765-1:1988; ISO 6383-2:1983 |
| Frozen food lamination | EU 10/2011 Annex I; FDA 21 CFR 177.1520; EC 2023/2006 | ISO 10364:2015; ISO 8296:2003 |
| Stretch hood logistics film | EU 94/62/EC Annex II; REACH Art. 33 | ISO 527-3:2018; ISO 7765-1:1988; ISO 8295:1995 |
| Greenhouse cover film | REACH Art. 33; EU 1272/2008 CLP | ISO 4892-2:2013; ISO 527-3:2018; ISO 14782:2021; ISO 9050:2003 |
Where a pallet unitisation line switches from polyethylene shrink film to stretch hood film, FG 306 A is processed on a three-layer blown film line at a blow-up ratio of 3.0:1 to 4.0:1 and a frost line height of 800–1,000 mm, producing tubular film of 100–150 µm that is stretched over the load by counter-rotating brush rollers. The resin is blended with 20–30 wt% LDPE or mLLDPE to increase melt strength and reduce bubble flutter. Die gap is set at 2.2 mm to lower shear stress, because the high blow-up ratio and large bubble diameter would otherwise generate circumferential gauge bands. Tensile behaviour is evaluated on 100 µm specimens by ISO 527-3:2018 at 500 mm/min; the film must exhibit longitudinal strain capability above 400% and sufficient recovery to maintain load containment after 30 min. Dart impact by ISO 7765-1:1988 is set above 400 g because the film contacts sharp pallet corners during the stretching cycle. MD tear resistance by ISO 6383-2:1983 is maintained above 200 g. Film-to-film coefficient of friction measured by ISO 8295:1995 is held at 0.25–0.35 to allow stacking without excessive pallet slip. The terminal product is a reusable or single-trip pallet hood used in chemical bag logistics. Industrial packaging compliance is evaluated under the EU Packaging and Packaging Waste Directive 94/62/EC, Annex II, and REACH Article 33 for SVHC content above 0.1% by mass.
Production-scale experience with stretch hood lines shows that film weight variation is the largest source of load containment failure, not tensile strength. At a bubble diameter of 1,400 mm, a temperature differential of 3°C across the die creates a thickness variation of ±8%, which is sufficient to produce localised overstretch and corner puncture. The remedy is to maintain die body temperature uniformity within ±1°C and to use a segmented air ring with differential cooling zones around the circumference. In addition, the blown line should not be stopped for more than 10 min with molten FG 306 A in the die because oxidation at the die lip creates carbonaceous specks that appear as black inclusions in the pallet hood. Start-up after downtime requires purging with low-density polyethylene until the melt pressure stabilises within ±5 bar of the previous running pressure.
Because greenhouse film loses tensile strength through UV stabiliser depletion, extrusion of FG 306 A into multi-season cover film requires a HALS/UV package at 8–10 wt% and an EVA or metallocene plastomer at 8–12 wt% to lower the minimum sealing temperature for tunnel canopies. The blown film line uses a die diameter of 250–400 mm, a die gap of 1.8–2.0 mm, and a blow-up ratio of 2.0:1 to 2.6:1. The desired optical performance is a photosynthetically active radiation transmission above 85%, measured by ISO 9050:2003 or ASTM D1003-21 for total transmittance, and a haze value between 15% and 25% by ISO 14782:2021. FG 306 A’s base crystallinity is adjusted through a low-density carrier masterbatch to a compounded density of 0.921–0.923 g/cm³, which controls light diffusion without forming large spherulites that would reduce tear resistance. Mechanical retention after accelerated weathering is measured by tensile elongation at break according to ISO 527-3:2018; a drop below 50% of the unexposed value indicates UV stabiliser depletion. The terminal product is a 150–200 µm greenhouse cover with a service-life target of 3–5 seasons.
Mineral filler addition for infrared retention must not exceed 12 wt%. At higher filler loading, the bubble stiffness increases and dart impact by ISO 7765-1:1988 falls below 300 g, while tear propagation by ISO 6383-2:1983 becomes directionally unstable. Film processors should maintain the extruder melt temperature below 240°C because the combination of HALS, filler carrier waxes and EVA can generate acidic volatiles above this threshold, causing die corrosion and condensation on the air ring. If anti-drip properties are required, a non-ionic glycerol ester additive at 0.5–1.0% is used, but it accelerates surface bloom and reduces wetting tension; corona treatment for printable covers must be delayed until after the anti-drip migration has stabilised at 72 h post-extrusion. Published data for the infrared retention coefficient of FG 306 A in a greenhouse formulation is limited; trial validation on the specific blown line with 1,000 h xenon-arc exposure to ISO 4892-2:2013 is required before multi-season field placement.
Competitive Versalis Clearflex® FG 306 A Film Grade LLDPE prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Versalis Clearflex FG 306 A is classified as a linear low-density polyethylene film grade. The resin is specified for blown film and cast film conversion where a nominal density of 0.918 g/cm3 and a melt flow rate of 1.0 g/10 min under ISO 1133-1:2022 conditions must be matched to bubble stability, seal initiation, dart impact, and optical clarity. The designation FG 306 A identifies the material as a film-grade polyethylene with controlled short-chain branching; it is distinct from high-pressure LDPE homopolymers and from metallocene LLDPE grades used in the same gauge range.
The grade is introduced into coextruded webs for form-fill-seal packaging, lamination film, and thin-gauge protective packaging. In these applications the primary processing challenge is not plastication but the stability of the molten bubble or cast web as the polymer exits the die. Linear low-density polyethylene has lower melt extension than long-chain-branched LDPE, so die gap, blow-up ratio, frost-line height, and take-off speed must be set to limit draw resonance and gauge variation. FG 306 A is typically chosen when the converter needs a lower seal initiation temperature than LDPE but does not require the extreme dart impact and hot-tack performance of a metallocene C6 or C8 copolymer.
Manufacturer certification for Clearflex FG 306 A is based on density measured according to ISO 1183-1 and melt mass-flow rate measured with a 2.16 kg load at 190 °C under ISO 1133-1:2022. The nominal density of 0.918 g/cm3 places the material in the lower density segment for linear low-density polyethylene film grades, which typically spans 0.915 g/cm3 to 0.925 g/cm3. The melt flow rate of 1.0 g/10 min is an intermediate value for blown film extrusion; it provides sufficient melt strength for bubble formation while limiting screw torque and melt temperature rise on grooved-feed extruders.
Density and melt flow rate do not fully define film behavior. Molecular weight distribution, comonomer length, and additive package control shear thinning, melt extension, blocking, and slip. Differential scanning calorimetry according to ISO 11357-3 on comparable 0.918 g/cm3 LLDPE film resins usually indicates a peak melting temperature in the 119–126 °C range and a crystallization temperature of 104–110 °C during controlled cooling. These thermal transitions establish the lower sealing boundary and the recommended barrel profile. Published grade-specific thermal data for FG 306 A are limited in open literature; the ranges cited here are industrial values for LLDPE of equivalent density and melt flow, not certified lot values.
| Parameter | Standard or method | Typical value or range | Restriction on use |
|---|---|---|---|
| Density | ISO 1183-1 | 0.918 g/cm3 | Lot certificate value controls; immersion method may vary by 0.0005 g/cm3 |
| Melt flow rate | ISO 1133-1:2022 | 1.0 g/10 min | 190 °C, 2.16 kg load |
| Melting peak | ISO 11357-3 | 119–126 °C | Second heating, 10 K/min |
| Haze | ISO 14782 | 3–8 % at 40 µm | Depends on antiblock, blow-up ratio, and frost line |
| Seal initiation temperature | ASTM F88 | 95–105 °C on 40 µm blown film | Seal bar pressure 2.8 bar, dwell 0.5 s |
On a grooved-feed single-screw extruder with a 30:1 L/D barrier screw, the material is commonly processed with a barrel profile beginning at 170 °C at the feed throat and rising to 210–215 °C in the metering section. Adapter and die zones are set at 220–230 °C to reduce melt fracture. The melt temperature should be held below 240 °C during steady-state operation. Above 240 °C, LLDPE grades with 0.918 g/cm3 density undergo oxidative chain scission at a rate that increases gel counts and reduces dart impact; this effect is measurable on a film line as an increase in specks per square meter after 15–20 min of residence at elevated temperature. Melt pressure at the breaker plate on a clean 60/80/100 mesh pack is typically below 35 MPa. A rise above 45 MPa indicates screen blinding or inadequate melt temperature and should be corrected before film optics degrade.
Die gaps of 1.6–2.4 mm are used for gauges above 20 µm. For thin webs below 15 µm, the die gap is usually reduced to 1.0–1.2 mm to impose higher shear and reduce molecular orientation in the machine direction. Blow-up ratio is set between 2.2:1 and 2.8:1. Frost-line height between 300 mm and 600 mm from the die face provides a balance between transverse direction tear and optical clarity. Internal bubble cooling is required when specific output exceeds approximately 1.2 kg/h per millimetre of die circumference; without internal cooling, bubble flapping and gauge banding above ±5 % are commonly observed on conventional air rings.
Cast film lines running the grade at 20–30 µm lamination webs typically use a flat die with 250–300 mm width and chill roll temperature of 18–25 °C. The resin is drawn down over a 20–40 mm air gap. Chill roll temperature below 15 °C can induce surface condensation and haze; above 30 °C lowers quench rate and increases film blocking. On a 90 mm extruder with a 2.4 m die, line speeds above 150 m/min can be achieved only when the die gap and air knife are optimized; higher speeds introduce gauge bands exceeding ±5 %.
The most significant difference between FG 306 A and a high-pressure LDPE homopolymer is the absence of long-chain branching. This structural feature reduces shear sensitivity and melt extension but increases solid-state puncture resistance. In blown film of 25–40 µm, a 0.918 g/cm3 LLDPE commonly exhibits dart impact values under ASTM D1709 between 80 g and 130 g, while an LDPE homopolymer of equivalent melt flow often falls below 60 g. Machine-direction Elmendorf tear according to ASTM D1922 is commonly 20–40 g/25 µm, and transverse-direction tear is 40–80 g/25 µm. These are not certified limits for FG 306 A; they are industrial ranges for the film class and must be verified on the specific line configuration.
Against a butene-based C4-LLDPE of the same density and melt flow rate, FG 306 A generally shows comparable seal initiation but improved gel consistency and optical quality, because the additive package and polymerization control limit the formation of high-molecular-weight fractions and oxidized gels. Against a hexene- or octene-based metallocene LLDPE, the grade typically exhibits a seal initiation temperature 5–15 °C higher and lower dart impact at equal gauge, but it provides wider bubble stability and lower screw torque on older extruders that lack high-shear mixing elements. The comonomer type also influences environmental stress cracking resistance measured under ASTM D1693; C6 and C8 copolymers usually outperform butene-based LLDPE in slow crack growth testing, while FG 306 A is selected when seal performance and processability are weighted more heavily than ultimate ESC resistance.
Optical haze in 40 µm blown film is typically between 3 % and 8 % when measured according to ISO 14782. Gloss at 60 ° measured by ASTM D2457 usually falls between 60 GU and 80 GU. These values are controlled more by die state, frost-line height, and antioxidant package than by density alone. On a line with a dirty die lip or excessively high melt temperature, haze can rise above 12 % even when the resin is within specification.
On vertical form-fill-seal machines, sealing jaws operating at 115–130 °C with dwell times of 0.3–0.5 s require hot-tack strength above 2.0 N/15 mm to prevent pouch opening before the seal solidifies. The seal initiation window of FG 306 A allows cycle rates up to 60 pouches/min on conventional rotary sealers, but the actual maximum is determined by jaw alignment, film slip additive, and package geometry. Hot-tack testing under ASTM F1921 with a 0.5 s seal bar dwell shows a typical maximum hot-tack window between 100 °C and 120 °C. Films that must survive hot-filled liquids require a broader hot-tack plateau, which may favor a metallocene C6 grade; FG 306 A is therefore placed where moderate hot-tack and lower resin cost are required.
Downgauging to 10–12 µm changes the dominant failure mode from tensile yield to puncture and tear propagation. At gauges below 12 µm, dart impact measured under ASTM D1709 commonly falls below 60 g, and trouser tear testing under ASTM D1938 becomes a more reliable discriminator of converting performance than Elmendorf tear. Seal bar temperature must be reduced by 5–10 °C to avoid burn-through, while dwell may need to increase to 0.4–0.6 s to maintain seal strength above 2.0 N/15 mm. This operational window is narrow because the heat transferred to the seal area at 10 µm is no longer buffered by the thermal mass of the film; small variations in jaw temperature of ±3 °C can shift the seal from cohesive failure to scorch marks.
Blocking becomes a critical limitation at thin gauges. If the coefficient of friction measured under ISO 8295 exceeds 0.35, the web will not slide over forming shoulders without wrinkling. The additive system of FG 306 A is intended to maintain coefficient of friction in the 0.10–0.25 range at 23 °C and 50 % relative humidity. Corona treatment above 42 mN/m can raise coefficient of friction by oxidizing the surface and increasing polar interactions; for lamination structures, treatment is therefore limited to the web face that will receive adhesive, not the slip-treated heat-seal layer.
Food-contact conformity for FG 306 A must be verified against the final film structure because additives, printing inks, and lamination adhesives alter overall migration behavior. The resin may be evaluated under FDA 21 CFR 177.1520 for olefin polymers and under Commission Regulation (EU) No 10/2011 for plastic materials intended to contact food. The final article is subject to overall migration limits of 10 mg/dm2 for general food contact, with specific migration limits applied to the additive package. REACH registration obligations for the polymer substance rest with the manufacturer, but downstream users must document the presence of any substances of very high concern in the converted article. RoHS Directive 2011/65/EU restrictions on lead, mercury, cadmium, hexavalent chromium, PBB, and PBDE are not generally problematic in virgin polyethylene film, but recycled content or masterbatch colorants can introduce non-compliant elements.
| Framework | Standard or clause | Assessment note |
|---|---|---|
| US food contact | FDA 21 CFR 177.1520 | Olefin polymer may be used subject to extractable fraction and end-use limitations; converter must verify finished article conditions of use |
| EU food contact | EU 10/2011 | Overall migration 10 mg/dm2; specific migration limits are formulation-dependent and require testing on the final film |
| Chemical registration | REACH | Polymer is exempt from registration but downstream article obligations apply if SVHC content exceeds 0.1 % w/w |
| Hazardous substances | RoHS 2011/65/EU | Virgin resin is typically below cadmium, lead, mercury, and hexavalent chromium limits; recycled content must be validated |
| Biodegradation or compostability | EN 13432 | Not applicable to non-biodegradable LLDPE; do not label FG 306 A as compostable |