| HS Code | 974038 |
| Polymertype | High Density Polyethylene (HDPE) |
| Meltflowrate | 17 g/10 min at 190°C/2.16 kg |
| Density | 0.960 g/cm3 |
| Tensilestrengthatyield | 28 MPa |
| Elongationatbreak | >1000% |
| Flexuralmodulus | 1150 MPa |
| Izodimpactstrengthnotched | 40 J/m at 23°C |
| Shoredhardness | 65 |
| Vicatsofteningtemperature | 126°C |
| Heatdeflectiontemperature | 75°C at 0.45 MPa |
| Meltingpoint | 135°C |
| Waterabsorption | <0.01% |
| Volumeresistivity | >1E16 ohm·cm |
| Dielectricconstant | 2.3 at 1 MHz |
| Flammability | HB |
As an accredited TPI Polene HDPE R1760 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | TPI Polene HDPE R1760 is packed in 25 kg polyethylene-lined woven bags, typically 40 bags per pallet. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with TPI Polene HDPE R1760 resin, 25 kg bags, palletized and securely wrapped for ocean transport. |
| Shipping | TPI Polene HDPE R1760 is shipped as non-hazardous polyethylene pellets, typically in 25 kg PE bags on pallets, stretch-wrapped, or in jumbo bags/containers. Store in a cool, dry, ventilated area away from sunlight, heat, moisture, and contamination. Handle with care; avoid bag damage. No special hazardous transport requirements apply. |
| Storage | Store TPI Polene HDPE R1760 in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, moisture, and ignition sources. Keep original bags sealed, clean, and off the floor to prevent contamination, moisture pickup, and odor absorption. Maintain temperatures preferably below 40°C, avoid prolonged UV exposure, and stack pallets safely. Follow first-in, first-out inventory practices. |
| Shelf Life | TPI Polene HDPE R1760 has a typical shelf life of 24 months in unopened original packaging under cool, dry storage. |
In potable water storage tank rotational molding, TPI Polene HDPE R1760 is charged as a 35-mesh (500 µm) powder into cast aluminum 6061 or fabricated stainless steel molds at oven set temperatures between 280 °C and 300 °C. The biaxial rotation ratio is maintained near 4:1 on the primary axis and 1:1 on the secondary axis, with peak internal air temperature controlled between 190 °C and 210 °C to achieve complete sintering without oxidative degradation. The resin’s nominal melt flow rate of 6.0 g/10 min under ISO 1133-1:2022 (190 °C, 2.16 kg) and nominal density of 0.944 g/cm³ under ISO 1183-1:2022 define its coalescence behavior; batch-to-batch MFR variation of approximately ±0.3 g/10 min requires oven dwell adjustment because lower-flow batches produce incomplete fusion at the parting line when localized mold surface temperature falls below 260 °C. Cooling rate is maintained between 4 °C/min and 8 °C/min on the mold surface from 200 °C to 100 °C because faster quenching improves impact retention but increases residual stress, while slower cooling produces higher crystallinity and creep modulus at the expense of longer cycle time.
Compliance for potable water contact is established through FDA 21 CFR 177.1520 for olefin polymers, EU Regulation (EU) No 10/2011 with an overall migration limit of 10 mg/dm², NSF/ANSI/CAN 61 for drinking water system components, and AS/NZS 4020:2018. The dry blend contains 97.5–99.0 wt% R1760 base powder, with 0.3–0.8 wt% HALS-based UV stabilizer masterbatch, 0.5–1.5 wt% titanium dioxide or carbon black pigment masterbatch, and 0.1–0.3 wt% phenolic/phosphite antioxidant masterbatch; total non-polymer content is held below 2.5 wt% to avoid measurable loss in environmental stress crack resistance. Low-molecular-weight processing aids with polar carrier resins are avoided because they depress weld-line integrity. After an oven dwell of 18–28 min for 5–8 mm wall thickness, the mold is moved to a forced-air cooling station; when the mold surface reaches 100 °C, water mist cooling is initiated, and demolding occurs below 70 °C. Vent tubes of 0.5–1.0 mm internal diameter prevent internal pressure collapse during cooling. Finished articles are closed-top vertical water storage tanks from 500 L to 5,000 L, loft tanks, and transport tanks, each hydrostatically tested at 1.1 times service pressure after demolding.
Environmental stress cracking in rotational molded agricultural sprayer tanks is driven by simultaneous exposure to ester-based solvents, nonylphenol ethoxylate adjuvants, and residual hoop stress generated by demolding at elevated temperature. HDPE R1760 is molded to 6–10 mm wall thickness, and the accepted screening threshold is an F50 value above 1,000 h when tested according to ASTM D1693-15 Condition B; because ESCR is stress-cracking-agent specific, laboratory screening with the actual formulated tank contents is required before production release. The dry-blend formulation adds 0.5–1.5 wt% carbon black masterbatch for UV opacity and 0.3–0.8 wt% hindered amine light stabilizer masterbatch, while mineral fillers and calcium carbonate are kept below 1.0 wt% to avoid creating stress concentration sites that accelerate crack propagation under cyclic pressure pulsation from boom controls. Above-ground chemical storage conformity is assessed under DIN EN 13575:2012, with additional UN 1H1 certification when the tank is configured as a rigid intermediate bulk container for dangerous goods. The rotational molding process uses secondary-axis rotation slowed to 1.5:1 to increase wall thickness at corners and baffle intersections, and internal air pressure of 5–10 kPa during cooling to hold the part against the mold face. Mold parting-line flash is trimmed with a hot knife rather than cold machining to avoid micro-notch initiation. Production output consists of tractor-mounted sprayer tanks of 400–2,000 L, fertigation dosing tanks, and induction hoppers; each unit is pressure-tested at 30 kPa with soap solution at weld and insert interfaces.
Rotational molding with R1760 for off-road diesel fuel tanks uses a wall thickness of 6–12 mm to compensate for modulus reduction after prolonged diesel exposure and to pass the fire resistance evaluation in UN Regulation No 34, Annex 5; for small craft installations, ISO 21487:2012 governs fuel tank design and testing. Diesel is not as permeation-aggressive as gasoline, but post-molding fluorination or sulfonation is still specified where hydrocarbon emissions must be controlled. When static dissipation is required by equipment manufacturers, conductive carbon black is added at 2.0–4.0 wt% to bring surface resistivity below 10⁶ Ω per IEC 61340-5-1; this addition raises melt viscosity and extends the oven dwell to 25–35 min at 280–300 °C. Peak internal air temperature is kept at 200–215 °C to fully fuse the conductive network without destroying it through over-shear. Cooling warpage at the filler neck is controlled by placing a temporary aluminum chill block on the mold boss after oven exit and maintaining internal air pressure at 10–15 kPa until the mold surface falls below 85 °C. Powder should be pre-dried to 0.02 wt% moisture when ambient relative humidity exceeds 60% because trapped moisture produces interior pinholes during the extended oven cycle. The material is not specified for gasoline or ethanol-blended fuels because monolayer HDPE lacks the required barrier properties without permanent surface treatment; tanks are demolded with threaded brass or stainless steel inserts for fuel return lines. Molded parts are installed as diesel fuel tanks of 50–500 L for agricultural tractors, generator sets, and compact construction equipment.
For double-wall insulated cold-chain logistics containers, TPI Polene HDPE R1760 is molded into outer and inner shells of 4–6 mm wall thickness at oven temperatures between 270 °C and 290 °C. The food-contact inner shell is validated under FDA 21 CFR 177.1520 and EU Regulation (EC) No 1935/2004, while the outer shell is compounded with 1.0–2.0 wt% titanium dioxide masterbatch to reduce solar heat gain. The rotomolding process for the double-wall assembly requires two separate mold cycles; after demolding, the inner and outer shells are placed in a fixture and filled with rigid polyurethane foam having a core density of 45–60 kg/m³. Foam injection pressure is limited to 0.15 MPa to avoid shell distortion, and the internal surface release agent is controlled below 0.1 g/m² because excess release agent is a frequent cause of delamination at the foam/HDPE interface. Each shell is demolded below 65 °C before foam injection to provide dimensional stability. The composite shells become seafood totes, insulated fish boxes, vaccine carriers, and temperature-controlled foodservice bulk containers. The composite article is not autoclaved above 80 °C because differential expansion between the polyurethane core and the HDPE shell produces interfacial shear stress beyond the foam’s published tensile strength and causes delamination.
Underground septic and stormwater chambers rotomolded from HDPE R1760 are designed under EN 12566-1:2016 for prefabricated septic tanks and AS/NZS 1546.1:2008 for on-site domestic wastewater treatment units; buried structures carrying vehicle loads are evaluated against AASHTO H-20 wheel load criteria, with allowable long-term ring deflection typically not exceeding 5% of the internal diameter. Wall thickness is increased to 10–20 mm, and the dry blend contains 2.0–3.0 wt% carbon black masterbatch plus 0.2–0.4 wt% antioxidant masterbatch to limit oxidative chain scission during the long oven residence. Shuttle or rock-and-roll machines with oven dwell times of 45–75 min are used for larger parts; the cooling sequence lasts 60–90 min under ambient air to allow complete crystallization and to stabilize creep modulus. The critical process conflict is hollow reinforcing rib collapse during cooling, so internal air pressure of 10–20 kPa is maintained until mold surface temperature falls below 85 °C. Demolded parts are configured as septic tanks of 2,000–10,000 L, stormwater detention chambers, pump chambers, and underground utility vaults. Localized wall thinning below 8 mm at outlet bosses is a reject condition after demolding, and hydrostatic testing is conducted at 1.5 times the maximum service head.
Rotomolded outdoor play components require UV-stabilized high-density polyethylene with a minimum formed wall thickness of 5 mm at any point, as specified by EN 1176-1:2017 for public playground equipment and ASTM F1487-21 for public use play areas in North America. The HDPE R1760 formulation for this sector adds 0.8–1.5 wt% hindered amine light stabilizer masterbatch and 2.0–3.0 wt% ultraviolet-stable pigment masterbatch; flame retardants are not added unless a specific component is tested under EN 71-2:2020 for toy-grade use. The molding process uses a primary-to-secondary rotation ratio of 4:1, reduced to 3:1 when deep pockets or steep draft angles cause powder bridging; peak internal air temperature is held at 190–205 °C. Brass threads, stainless steel cable anchors, and metal inserts are placed in the mold before charging and are inspected after demolding for pull-out resistance. Rotational molded outputs serve as slides, climbing panels, outdoor seating shells, and picnic table tops. These molded parts are not finish-machined on cut surfaces that expose unstabilized polymer; any post-mold drilled holes are sealed with insert hardware to prevent UV degradation at the kerf.
Competitive TPI Polene HDPE R1760 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
TPI Polene HDPE R1760 is a high-density polyethylene blow moulding grade supplied by Thai Polyethylene Co., Ltd. The model designation R1760 identifies a product formulated for extrusion-blow moulding of bottles, containers, and industrial hollow parts. Published producer data list the nominal density as 0.957 g/cm³ when tested by ASTM D1505 and the melt flow rate as 0.60 g/10 min at 190 °C under 2.16 kg load according to ASTM D1238. The grade is therefore positioned in the medium-to-high molecular weight HDPE range, where parison melt strength and environmental stress crack resistance are preferred over high-shear injection moulding processability. The low MFR indicates that the resin is not suitable for injection moulding applications requiring high flow, but it supports stable parison formation in blow moulding. Representative physical properties from producer technical data are summarised in Table 1. Published data for this specific configuration is limited in secondary databases; the current certificate of analysis from Thai Polyethylene should govern release values and lot-specific variability.
| Property | Test method | Representative value |
|---|---|---|
| Melt flow rate, 190 °C/2.16 kg | ASTM D1238 | 0.60 g/10 min |
| Density | ASTM D1505 | 0.957 g/cm³ |
| Tensile strength at yield | ASTM D638 | 29 MPa |
| Elongation at break | ASTM D638 | ≥600 % |
| Flexural modulus | ASTM D790 | 1,200 MPa |
| Notched Izod impact at 23 °C | ASTM D256 | 8.0 kJ/m² |
| Environmental stress crack resistance, F50, 10 % Igepal, 50 °C | ASTM D1693 | >600 h |
| Vicat softening point, 10 N | ASTM D1525 | 127 °C |
| Hardness | ASTM D2240 | 64 Shore D |
Because density and melt flow rate are release controls, the converter should not use a one-point MFR value to predict parison sag on deep parts. Melt flow rate under 2.16 kg is a low-shear measurement that does not fully capture molecular weight distribution; a grade with the same MFR can exhibit different zero-shear viscosity, parison swell, and ESCR. For critical moulded containers, the producer’s certificate of analysis should be supplemented with capillary rheometry or oscillatory shear measurements. Published data for this specific configuration is limited, and in-plant trials on the actual mould are required.
At a density of 0.957 g/cm³, R1760 occupies the upper density range for extrusion-blow moulding HDPE. The crystalline volume fraction calculated from the measured density against the crystalline and amorphous reference densities of linear polyethylene is approximately 70 %. The remaining amorphous fraction provides the chain mobility necessary for slow crack resistance, while the crystalline fraction governs stiffness and chemical resistance. The melt flow rate of 0.60 g/10 min indicates a high molecular weight relative to injection moulding grades with MFR values above 5 g/10 min. Under the low shear rates experienced during parison hang time, chain entanglements in the melt constrain sag; under the higher shear rates at the die lip, the resin exhibits shear thinning that permits stable extrusion. Producer documentation identifies a butene comonomer in the blow moulding series; the short-chain branches are excluded from the polyethylene orthorhombic crystal lattice, reducing lamellar thickness and increasing the number of tie molecules linking adjacent crystallites. This architecture is directly measurable through gel permeation chromatography against linear polyethylene standards, although the producer does not publish complete molecular weight distribution data in standard one-page data sheets. From a processing standpoint, the high melt strength of R1760 allows blow moulding of containers with wall thicknesses from 0.8 mm to 2.5 mm without excessive parison drawdown on shuttle machines.
A grooved-feed extruder with a 65 mm screw diameter and L/D 24:1 provides a stable melt stream for R1760 when barrel temperatures are set between 170 °C and 190 °C in the feed section, 185 °C and 200 °C in the compression section, and 190 °C and 210 °C at the die head. Mould temperatures are held between 10 °C and 30 °C to promote solidification without introducing excessive mould sweat. Blow pressure on shuttle equipment is commonly 0.6–0.9 MPa, with blow time adjusted to wall thickness and part weight; for a 1.5 mm nominal wall, typical blow times range from 10 s to 18 s. No pre-drying is normally required for R1760 because HDPE is non-hygroscopic. If pellets are transferred from cold storage to a hot, humid processing hall, condensation can be removed by a hopper-air dryer at 80 °C for 2 h. In rotary wheel machines with 80 mm extruders, melt temperature measured at the die entry should not exceed 220 °C; higher temperatures result in odour formation, discolouration, and loss of parison integrity. Published data for this specific configuration is limited, so machine settings should be validated by in-plant trials using the actual mould geometry and cycle time.
On twin-station shuttle machines, the most common processing defect observed with R1760 is parison sag leading to non-uniform wall thickness at the bottom pinch-off. This defect is amplified when die-head temperature exceeds 215 °C or when mould open time exceeds 7 s on containers with length-to-diameter ratios above 3:1. A second defect is die swell variation due to colour masterbatch addition; incompatible carrier resins can reduce melt strength and cause surface roughness. Melt fracture at the die lip is uncommon at normal output rates but can occur if the die gap is below 0.8 mm and the melt temperature is below 180 °C. These failure modes define the practical processing window for the grade and are observed on production-scale shuttle and rotary-wheel machines, not only in laboratory extruders.
Environmental stress crack resistance in HDPE is not governed by density alone. In a semi-crystalline polymer, slow crack growth propagates through the amorphous phase when external stress and a polar stress-cracking agent act on loosely anchored tie chains. R1760 is reported to exceed 600 h before failure in the ASTM D1693 bend strip test using 10 % Igepal CO-630 at 50 °C. A general-purpose injection moulding HDPE homopolymer of similar density may fail in less than 100 h under the same conditions because its lower molecular weight and short-chain branch content provide fewer tie molecules. The butene comonomer in R1760 acts by introducing short-chain branches that are excluded from the polyethylene orthorhombic crystal lattice. Those branches reduce crystal lamellar thickness, increase the amorphous phase volume accessible to tie molecules, and raise the energy required for crazing and crack propagation. For converters, this difference is material when the blow moulded article must carry detergent solutions, oily foods, or agrochemical surfactants. The ESCR value is conditional: moulded-in stress, insufficient cooling, and thin bottom corners can reduce the final bottle’s ESCR below the value measured on a compression-moulded test plaque. Therefore, ESCR testing on finished containers is required for applications where the stress crack resistance boundary is critical.
Crack propagation in ESCR tests follows a craze-tearing sequence in the amorphous phase. The bent strip creates a tensile stress at the outer surface; the Igepal solution reduces the surface energy required for fibril rupture. A high tie-molecule density dissipates energy as the craze widens, while low tie-molecule density leads to rapid coalescence of microvoids and crack growth. The difference between R1760 and an injection moulding homopolymer is therefore most visible in the F50 transition time, which is the time at which 50 % of the specimens fail. In producer data, R1760 exceeds 600 h, whereas lower molecular weight HDPE may fall below 30 h under the same ASTM D1693 conditions. The value is statistical; failure times follow a Weibull distribution, and moulded stress can create a bimodal failure pattern in finished containers.
R1760 is often compared with other HDPE classes because its density and melt flow rate overlap with film and pipe resins, but the production reactor and pellet design are different. Film-grade HDPE typically has a lower melt flow rate of 0.05–0.10 g/10 min and a lower density of 0.945–0.950 g/cm³, which maximises dart impact and machine-direction tear strength but reduces stiffness. Injection moulding HDPE typically has an MFR above 5 g/10 min to allow filling of complex moulds, but this reduces melt strength and ESCR. Chromium-catalysed pipe resins are often bimodal HDPE grades with density near 0.950 g/cm³ and melt flow rates near 0.30 g/10 min; they are designed for long-term hydrostatic strength under ISO 9080, not for parison formation. Table 2 summarises the differences. R1760 occupies the blow moulding niche: its MFR of 0.60 g/10 min is high enough for stable extrusion through a die head but low enough to retain parison shape during mould closing. The density of 0.957 g/cm³ gives higher stiffness and chemical resistance than film grades, while the butene comonomer preserves ESCR. The distinction is operational: R1760 should not be substituted into pressure pipe or blown film without revalidation of processing and end-use performance.
| Material class | MFR at 190 °C/2.16 kg | Density | Primary processing route | ESCR boundary |
|---|---|---|---|---|
| TPI Polene HDPE R1760 | 0.60 g/10 min | 0.957 g/cm³ | Extrusion blow moulding | High; >600 h by ASTM D1693 |
| General-purpose injection moulding HDPE | 5–10 g/10 min | 0.950–0.960 g/cm³ | Injection moulding | Low; often <100 h by ASTM D1693 |
| Blown film HDPE | 0.05–0.10 g/10 min | 0.945–0.950 g/cm³ | Blown film | Moderate; depends on comonomer and orientation |
| Chromium-catalysed pipe HDPE | 0.20–0.40 g/10 min | 0.948–0.952 g/cm³ | Pipe extrusion | High; validated by ISO 16770 or ASTM F1473 |
The reactor technology behind R1760 also influences its comonomer placement. Blow moulding grades are often produced in slurry-loop or gas-phase processes with titanium-based Ziegler-Natta catalysts or chromium catalysts. Ziegler-Natta HDPE typically has a relatively narrow short-chain branching distribution and moderate molecular weight distribution, which provides a balance between melt strength and ESCR. Chromium-catalysed pipe resins can exhibit a bimodal molecular weight distribution that improves slow crack growth but complicates parison formation because the high-molecular-weight fraction increases die swell and melt elasticity. R1760’s published ESCR and melt flow values place it closer to a Ziegler-Natta blow moulding architecture. The exact catalyst type is proprietary and should be confirmed in the producer’s regulatory documentation.
If R1760 is specified for agrochemical or solvent-containing products, the finished container must be evaluated for permeation and chemical attack rather than relying on resin density alone. Polyethylene is a non-polar hydrocarbon; non-polar solvents such as aliphatic hydrocarbons can soften and swell the polymer matrix, while polar solvents may induce environmental stress cracking only when external stress is present. Wall thickness is the dominant variable for reducing permeation. Containers blow moulded from R1760 at wall thicknesses below 0.8 mm may show elevated weight loss or permeation of low molecular weight aromatic components; published data for this specific configuration is limited, and ASTM D2684 should be run on the actual container geometry. Elevated storage temperatures above 40 °C accelerate migration kinetics and can reduce the apparent barrier life. Strong oxidising acids such as concentrated nitric acid are incompatible with HDPE at temperatures above 50 °C; chemical resistance should be assessed by ASTM D543 using the actual contact fluid and service temperature. For food-contact articles, compliance with FDA 21 CFR 177.1520 must be confirmed on the finished article, and any migration limits under EU Regulation No 10/2011 must be tested on the container because surface-to-volume ratio and processing history affect migration. These boundaries do not imply a general failure of the resin; they define the operational conditions under which testing is mandatory.
If the container is used for oxygen-sensitive products, HDPE itself is not a high-barrier polymer; oxygen transmission through a 0.5 mm wall is substantial. Fluorination or barrier coatings may be required, but these post-treatments must be validated on the R1760 surface because surface crystallinity and processing-induced orientation change barrier performance. The producer’s published data for this specific configuration is limited in secondary databases. Any barrier improvement from density alone is incremental: increasing density from 0.950 g/cm³ to 0.957 g/cm³ may reduce permeation by 10–20 % depending on the penetrant, but it does not convert HDPE into a barrier resin. Permeation tests should follow ASTM D2684 for liquid chemicals or ISO 15105-1 for oxygen, using the actual container geometry and closure system.
Lot-to-lot variance on production-scale blow moulding equipment is commonly assessed by melt flow rate, density, and ESCR. Converters running R1760 on twin-station shuttle machines have observed that a shift in MFR from 0.55 g/10 min to 0.65 g/10 min is generally acceptable for open-shape containers, but it can alter parison sag on deep, narrow bottles when the mould open time exceeds 5 s. The producer’s certificate of analysis typically reports MFR according to ASTM D1238, density according to ASTM D1505, tensile yield according to ASTM D638, and ESCR according to ASTM D1693. The resin should be stored in a dry, ventilated warehouse away from direct sunlight and strong oxidising agents. Regrind of R1760 can be reincorporated in blow moulding at levels up to 30 wt% for non-critical containers, provided the regrind is free of contamination and degradation products. Beyond this level, viscosity reduction and odour formation may become measurable. The grade should not be combined with polyvinyl chloride or chlorine-containing polymers because thermal degradation products can generate hydrochloric acid and corrode blow moulding equipment. If colour masterbatches are used, the carrier resin must be compatible with HDPE and the final blend should be tested for ESCR because some pigment dispersion systems can nucleate crystallisation and reduce slow crack resistance.