| HS Code | 680443 |
| Density | 0.964 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 8.0 g/10 min |
| Tensile Strength At Yield | 30 MPa |
| Tensile Elongation At Break | 500% |
| Flexural Modulus | 1.30 GPa |
| Izod Impact Strength Notched | 4.0 kJ/m² |
| Shore D Hardness | 66 |
| Vicat Softening Point | 125°C |
| Heat Deflection Temperature 0 45 Mpa | 72°C |
| Melting Point | 133°C |
| Water Absorption | <0.01% |
| Linear Mold Shrinkage | 1.5–3.0% |
| Thermal Conductivity | 0.45 W/m·K |
| Dielectric Constant | 2.3 |
| Volume Resistivity | >1.0E15 ohm·cm |
| Flammability | UL94 HB |
As an accredited TPC (Japan) HDPE KXW64N factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | TPC (Japan) HDPE KXW64N is supplied in 25 kg net-weight multi-wall paper bags, palletized and shrink-wrapped. |
| Container Loading (20′ FCL) | Container loading: TPC (Japan) HDPE KXW64N in 20′ FCL dry container; 25 kg bags palletized, securely stowed, moisture-protected, maximum payload. |
| Shipping | Not restricted: HDPE (high-density polyethylene) KXW64N, TPC Japan, non-hazardous polymer resin. Transport in clean, dry containers. Packed in 25 kg bags, jumbo bags, or bulk. Store away from heat, moisture, UV, and contamination. No special hazard labels required. Follow local transport regulations. Handle with care to avoid package damage. |
| Storage | Store TPC (Japan) HDPE KXW64N in a cool, dry, well-ventilated warehouse. Keep bags or containers tightly closed, off the floor, and away from direct sunlight, moisture, heat, ignition sources, and strong oxidizers. Avoid prolonged UV exposure and contamination. Stack securely to prevent package damage. Use clean handling equipment. Maintain ambient temperature; observe local regulations and manufacturer guidance. |
| Shelf Life | Typically 24 months when stored unopened in original packaging in a cool, dry, well-ventilated area away from direct sunlight. |
HDPE KXW64N (TPC Japan) is specified for injection molding lines where melt temperature is maintained between 190 °C and 230 °C and mold temperature is held at 10-40 °C. Typical certificates of analysis reference density 0.964 g/cm³ (ISO 1183-1) and melt flow rate 5.0 g/10 min (ISO 1133-1 at 190 °C/2.16 kg). Tensile yield strength is typically 28 MPa (ISO 527-2), flexural modulus 1,350 MPa (ISO 178), and notched Izod impact strength 6 kJ/m² at 23 °C (ISO 180/A). The resin should not be processed above 250 °C melt temperature; prolonged residence at that upper limit accelerates chain scission and generates low-molecular-weight fractions that increase odor in finished articles. Surface moisture from storage at relative humidity above 60% should be removed by hopper drying at 70-80 °C for 2 h; HDPE has negligible equilibrium moisture uptake, but condensation on cold pellets is the operational failure mode.
| Property | Test method | Typical value |
|---|---|---|
| Density | ISO 1183-1 | 0.964 g/cm³ |
| Melt flow rate | ISO 1133-1:2022 | 5.0 g/10 min |
| Tensile yield strength | ISO 527-2 | 28 MPa |
| Flexural modulus | ISO 178 | 1,350 MPa |
| Notched Izod impact at 23 °C | ISO 180/A | 6 kJ/m² |
In 5 L to 25 L open-head pail production, KXW64N is usually run at 100 phr resin with 2-4 phr carbon black masterbatch for UV stabilization and 0.5-1.0 phr fluoropolymer processing aid. Carbon black grades with particle size below 20 nm improve weatherability but raise melt viscosity by 3-5%, so dosing must be adjusted when a color concentrate is changed. The governing compliance framework for dangerous-goods pails is the UN Model Regulations Chapter 6.1, implemented through ADR/RID and the IMDG Code; packaging type 1H1 and 1H2 requires drop, leakproofness, hydraulic pressure, and stacking tests. Production equipment includes accumulator-assisted injection molding machines with clamp force from 650 t to 1,600 t, screw L/D 22:1-25:1, compression ratio 2.5:1-3.0:1, and hot-runner valve-gated manifolds. Melt temperature is held at 210-230 °C, mold temperature at 15-35 °C, and injection speed is set to fill 85-95% of the cavity before switch-over at a screw cushion of 8-12 mm. Cavity pressure at end of fill commonly reaches 45-60 MPa; when clamp force is insufficient or the parting line is worn, flash appears at the rim. Vent depth below 0.02 mm causes burn marks at the flow front and increases cavity pressure variability. Terminal products include open-head pails for coatings, adhesives, bulk food ingredients, and chemical intermediates; molded-in handle attachments are tested at 1.2 m drop height after conditioning at -18 °C for 24 h under ADR packaging instruction P001.
On logistic molding lines, KXW64N is compounded with 70-80 wt% virgin resin and 20-30 wt% clean in-house regrind; top-loaded additives are 2-3 phr UV masterbatch and 0.5-1.5 phr antistatic masterbatch where static-sensitive automotive or electronics packaging is handled. Loading certification for pallets references ISO 8611-1:2021 and ASTM D1185-20; distribution packaging must also comply with EU Packaging Directive 94/62/EC heavy-metal limits and REACH SVHC disclosure. Production is normally run on large injection molding machines with clamp force from 1,200 t to 2,800 t, melt temperature 205-225 °C, mold temperature 20-40 °C, and injection pressure of 80-110 MPa. For thick-section pallet decks, structural-foam or gas-assist molding with 0.5-1.0 wt% endothermic chemical blowing agent reduces sink marks and part mass by 8-15%. The critical failure mode is not yield strength but creep under static load; creep modulus is evaluated under ISO 899-2 at 40 °C. Terminal products include nestable crates, stack-nest distribution containers, automated warehouse totes, and euro-type pallets with nine-block or perimeter runners.
In high-cavitation closure tools, KXW64N experiences apparent wall shear rates above 10⁴ s⁻¹ at cold-runner gate diameters of 0.4-0.8 mm. The compound is formulated at 100 phr KXW64N with 1-2 phr slip masterbatch to control removal torque, 1-3 phr color masterbatch, and 0.05-0.15 phr acid scavenger. Oxygen-scavenger or barrier additives are not recommended because HDPE provides inadequate oxygen transmission-rate improvement without a multilayer structure. Food-contact closures require raw-material compliance with FDA 21 CFR 177.1520 and finished article verification under EU Regulation 10/2011, including overall migration below 10 mg/dm². Molding parameters are bounded: melt temperature 220-240 °C, hot-runner manifold temperature 230-245 °C, mold cooling temperature 8-15 °C, injection speed 150-250 mm/s, and back pressure 5-10 MPa. Short-shots occur when switch-over position is later than 8 mm, while gate blush appears at injection speeds above 300 mm/s in tools without cavity-pressure sensors. Terminal products include tamper-evident beverage closures, HDPE dispensing caps for dairy and condiments, and snap-fit overcaps for personal-care containers.
In pressure-bearing water-contact components, KXW64N is usually formulated at 100 phr resin with 0.2-0.35 phr hindered phenolic antioxidant and 0.1-0.2 phr phosphite process stabilizer; carbon black is added at 1-2 phr only when UV resistance is required, but the selected carbon black grade must not introduce polycyclic aromatic hydrocarbons above the limits in EU Regulation 10/2011. The relevant compliance pathway is NSF/ANSI/CAN 61:2023 for drinking water system components, supplemented by FDA 21 CFR 177.1520 for the resin and EC 1935/2004 for the food-contact framework. Molding uses melt temperatures at the lower end, 205-220 °C, because thermal degradation products raise aqueous extraction values; mold temperature is held at 30-50 °C to reduce weld-line weakness at the thread root. Terminal articles include whole-house filter sumps, under-sink reverse-osmosis membrane housings, and quick-connect fittings for polypropylene tubing. Published data for KXW64N in NSF-listed formulations is limited, so lot-specific extraction testing is required rather than extrapolation from generic HDPE certifications.
Because sidewall stock is routinely held below 0.8 mm, dairy and deli thin-wall containers place simultaneous demands on injection speed and mold cooling. The formulation is normally 100 phr KXW64N with 3-5 phr white masterbatch containing 50-60 wt% TiO₂ and 0.3-0.8 phr fluoropolymer processing aid to delay sharkskin at high linear speeds; silicone-based mold-release agents are minimized because they interfere with lid sealing. Compliance is governed by FDA 21 CFR 177.1520, EU Regulation 10/2011, and Commission Regulation EC 2023/2006 on good manufacturing practice for food-contact materials. Molding lines use high-speed injection machines with clamp force from 350 t to 650 t, accumulator-assisted injection, melt temperatures 215-235 °C, and mold temperatures 10-20 °C. Conformal cooling channels with 8-12 mm diameter reduce cycle time to 6-9 s in 24-48 cavity tools. Terminal products include injection-molded dairy tubs, deli containers, cold food cups, and tamper-evident food trays. The main process risk is gate freeze-off at wall thickness below 0.35 mm, which is addressed by raising melt temperature but not above 245 °C to avoid organoleptic failure in milk-contact applications.
At regrind fractions above 30 wt%, notched Izod impact under ISO 180/A declines by more than 15% and environmental stress-crack resistance under ASTM D1693 condition B drops below 20 h in some detergent solutions. Industrial storage totes and modular racking bins molded with KXW64N are therefore formulated with 0-30 wt% clean post-industrial regrind; UV masterbatch is added at 2-3 phr for outdoor or UV-sterilized environments. The compliance baseline is ISO 11469 resin identification, with EU Regulation 10/2011 applicable only when food residues are stored; general industrial use requires REACH registration statements and UL 94 HB when molded parts are used inside electrical enclosures. Production runs on medium- to high-clamp-force machines with melt temperature 210-225 °C, mold temperature 25-40 °C, and injection speed profiled to avoid jetting in thick boss areas. Gas-counterpressure molding or sequential valve gating is used for parts above 6 mm nominal wall to suppress sink. Terminal products include solid-wall storage totes, modular racking bins, e-commerce returnable totes, and clean-room-compatible component trays. Additive packages should avoid zinc stearate above 0.3 phr because plate-out on vent surfaces increases cleaning frequency.
Competitive TPC (Japan) HDPE KXW64N prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
TPC (Japan) HDPE KXW64N is a high-density polyethylene resin supplied as a pelletized commercial grade within the TPC (Japan) portfolio. The KXW64N suffix defines a specific density class, molecular weight architecture, and additive system, but the alphanumeric code itself is not a normative specification. The current TPC (Japan) technical datasheet and the accompanying lot certificate of analysis remain the controlling reference for release values. Published third-party data for this specific configuration is limited; therefore, process and performance parameters presented here are framed as class-typical intervals for high-molecular-weight HDPE extrusion grades and must not be read as KXW64N lot guarantees.
For high-density polyethylene extrusion grades, commercial specification is usually arranged around density, melt flow under two or more loads, tensile properties, flexural modulus, impact resistance, Vicat softening point, and environmental stress-crack resistance. When KXW64N is specified by a downstream converter, the following matrix provides the standard designations and class-typical HMW-HDPE intervals. The values are not a substitute for the KXW64N certificate of analysis.
| Property | Standard method | Class-typical interval | Verification requirement |
|---|---|---|---|
| Density at 23 °C | ISO 1183-1:2019 | 0.948–0.956 g/cm³ | Lot certificate of analysis |
| Melt flow rate at 190 °C/5 kg | ISO 1133-1:2022 | 0.20–0.50 g/10 min | Process control only |
| Melt flow rate at 190 °C/21.6 kg | ISO 1133-1:2022 | 8–12 g/10 min | High-load MFR |
| Flow-rate ratio | Derived from ISO 1133-1:2022 | 30–60 | Molecular weight breadth indicator |
| Tensile yield stress | ISO 527-2:2012 | 21–25 MPa | Type 1A specimen |
| Elongation at break | ISO 527-2:2012 | >600% | Test speed 50 mm/min |
| Flexural modulus | ISO 178:2019 | 700–900 MPa | Test speed 2 mm/min |
| Charpy notched impact at 23 °C | ISO 179-1/1eA | >20 kJ/m² or no break | Specimen type 1 |
| Vicat softening temperature A50 | ISO 306:2022 | 120–126 °C | Load 10 N |
| Environmental stress-crack resistance | ASTM D1693-21 | >100 h Condition B | Igepal concentration fixed by method |
Melt flow rate values should be measured after purging under conditions specified in ISO 1133-1:2022. The ratio between high-load MFR and lower-load MFR is used to infer the breadth of the molecular weight distribution. For KXW64N-class materials, a flow-rate ratio in the 30–60 range is typical of high-melt-strength extrusion resins, but exact ratio must be obtained from TPC (Japan).
Moisture uptake in HDPE is low, but surface condensation at high humidity is process-relevant. When storage or conveying ambient relative humidity exceeds 60%, pre-drying at 70–80 °C for 2–4 h in a desiccant hopper dryer is required. Residual moisture above 0.05% by mass produces splay, pinholing, and hydrolysis of any ester-based processing aids. Feed-throat temperature should be held below 40 °C. If water contact is confirmed by pressure rise in the first barrel zone or visual splay in sheet, drying should be extended rather than compensated by barrel temperature increase.
In blown film lines, KXW64N-class polymer is processed with die gaps from 1.2–2.0 mm, blow-up ratios between 2.0:1 and 4.0:1, and melt temperatures at the die of 195–210 °C. Frost-line height is adjusted to maintain bubble stability; excessive drawdown reduces impact strength. Dart impact resistance is measured under ASTM D1709A and Elmendorf tear under ASTM D1922. These values are geometry-dependent and cannot be inferred from tensile properties.
In production-scale extrusion on grooved-barrel single-screw extruders with screw diameters in the 45–75 mm range and L/D ratios from 24:1 to 33:1, melt pressure fluctuation above ±5% of setpoint indicates unstable solids conveying, screen-pack plugging, or temperature stratification in the die adapter. A barrel profile from 180 °C in the feed zone to 195 °C in the metering zone, with adapter and die at 200–210 °C, is typically maintained for high-melt-strength HDPE. If melt temperature at the adapter falls below 195 °C, surface melt fracture appears as sharkskin on the extrudate; if it rises above 220 °C, thermo-oxidative degradation forms gel particles and brown specks. Screen-pack differential pressure should be recorded at intervals not exceeding 8 h; a rise above 0.8–1.2 MPa during a 24 h campaign calls for screen change. The pressure transducer should be located no more than 10D upstream of the screen changer to detect porosity and filler agglomeration before dimensional instability occurs.
Sheet extrusion of KXW64N-class material requires polished chrome rolls with roll temperatures from 70–90 °C and gap settings from 0.5–2.0 mm. Thermoforming sag is controlled by melt strength; sheet surface defects from moisture are amplified at draw ratios above 2.5:1. Where carbon black masterbatch is introduced at let-down ratios from 4–6%, twin-screw compounding lines with L/D 44:1 and screw speed 300–600 rpm are used. Elevating screw speed above 600 rpm can raise melt temperature above 230 °C and accelerate degradation of the polymer matrix.
Where KXW64N is converted into pressure pipe, short-term yield stress and elongation are not sufficient for grade selection. Long-term hydrostatic strength is evaluated under ISO 9080:2022, and material classification under ISO 12162:2009 requires an extrapolated lower confidence limit. A PE100 designation demands 10 MPa hydrostatic strength at 20 °C and 50 years. If KXW64N is represented as a pipe material, the TPC (Japan) MRS value should be obtained from the manufacturer’s certification. Batch-to-batch variance in co-monomer distribution and carbon black dispersion influences slow crack growth resistance. Full-scale pipe testing under ISO 1167 and notched pipe testing under ISO 13479 are used to verify performance; single-point melt index or density measurements cannot replace these tests.
Differentiation among HDPE grades is driven by density, melt flow rate, flow-rate ratio, and additive package. High-MFR injection moulding HDPE may show MFR at 190 °C/2.16 kg in the 8–20 g/10 min range, whereas high-melt-strength extrusion grades such as KXW64N are supplied at fractional melt flow with higher high-load MFR. This creates a shear-thinning response that reduces sag in sheet, large-part blow moulding, and thick-wall pipe. Compared with low-density HDPE film grades of lower density, KXW64N-class resins exhibit higher flexural modulus and lower permeability but reduced environmental stress-crack resistance unless co-monomer placement is optimized. The selection between KXW64N and other TPC (Japan) grades should be made using capillary rheometry under ISO 11443 and ESCR data under ASTM D1693-21, not by nominal density alone.
For injection moulded caps or crates, the same KXW64N designation would be inappropriate unless the converter adjusts screw design and gate geometry. High shear rates above 10³ s⁻¹ in thin-wall injection moulding require lower viscosity than KXW64N-class extrusion grades usually provide. Published data for this specific configuration is limited; trials on a 100 t clamp-force injection moulding machine with melt temperature 200 °C and mould temperature 30 °C would be required to establish whether flow-length ratio meets the part design.
Regulatory conformity depends on the base resin and the exact additive package used by TPC (Japan). A grade designation alone does not establish legal compliance. The following matrix identifies the standards that purchasers must verify against the current manufacturer’s declaration.
| Requirement | Standard or reference | Typical condition | Verification boundary |
|---|---|---|---|
| Food contact | FDA 21 CFR 177.1520 | Olefin polymer base | Additive package dependent |
| EU food contact | Regulation (EU) No 10/2011 | Overall migration ≤10 mg/dm² | Annex I restrictions apply |
| REACH SVHC | Regulation (EC) No 1907/2006 | SVHC ≤0.1% w/w | Article 57 list |
| RoHS | Directive 2011/65/EU | Pb, Hg, Cd, Cr6+, PBB, PBDE ≤0.1% w/w | Exemptions may apply |
For potable water pipe, additional test requirements arise from chlorine resistance standards such as ASTM F2263 and national potable water approvals; these are application-specific and not covered by generic HDPE datasheet values. The absence of an explicit TPC (Japan) statement for a directive should be treated as non-verification.
KXW64N should not be exposed to melt temperatures above 230 °C for campaigns exceeding 1 h because chain scission and gel formation accelerate. Avoid combining KXW64N with amine-based or nitroxyl-based additive masterbatches unless oxidative induction time under ISO 11357-6 and long-term heat stability under ISO 4577 confirm compatibility. Do not process with residual moisture above 0.05%. Do not rely on short-term tensile data for pressure-pipe service. For outdoor exposure, carbon black concentrations of 2.0–2.5 wt% with mean aggregate size below 20 µm are typical for UV stabilization, but final concentration must follow the manufacturer’s specification.