| HS Code | 665886 |
| Density | 0.954 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 0.06 g/10 min |
| Tensile Strength At Yield | 28 MPa |
| Tensile Strength At Break | 35 MPa |
| Elongation At Break | 800% |
| Flexural Modulus | 1.10 GPa |
| Izod Notched Impact Strength | 0.50 J/cm |
| Shore D Hardness | 65 |
| Vicat Softening Temperature | 125°C |
| Melting Temperature | 130°C |
| Brittleness Temperature | -70°C |
| Thermal Conductivity | 0.35 W/m·K |
| Linear Thermal Expansion Coefficient | 120 µm/m·°C |
| Dielectric Constant | 2.3 |
| Dissipation Factor | 0.0002 |
| Volume Resistivity | 1.00E+15 ohm·cm |
| Dielectric Strength | 20 kV/mm |
| Water Absorption | 0.01% |
As an accredited TPC (Japan) HDPE KM660W factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | TPC (Japan) HDPE KM660W is typically supplied in 25 kg bags, 40 bags per pallet (1,000 kg). |
| Container Loading (20′ FCL) | 20′ FCL container loading: TPC Japan HDPE KM660W in 25 kg bags, palletized, stretch-wrapped, and secured for safe ocean shipment. |
| Shipping | TPC (Japan) HDPE KM660W is a non-hazardous high-density polyethylene resin. It is typically shipped in 25 kg bags or bulk bags, palletized and shrink-wrapped, in dry containers. Store cool, dry, ventilated, away from sunlight, heat, and moisture. Not regulated for transport. |
| Storage | Store TPC (Japan) HDPE KM660W in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and oxidizing agents. Keep original containers or bags closed, palletized, and off the floor to prevent moisture, dust, and contamination. Avoid prolonged UV exposure. Do not store near strong acids, bases, or solvents. Follow first-in, first-out stock rotation and local regulations/SDS recommendations. |
| Shelf Life | Shelf life is typically 24 months from manufacture when stored unopened in original packaging, dry, cool, and protected from direct sunlight. |
KM660W is a high-molecular-weight high-density polyethylene copolymer with a broad molecular weight distribution. Its melt-flow rate is typically below 0.5 g/10 min when measured under ISO 1133-1:2022 at 190 °C and 2.16 kg, and density is in the 0.950–0.955 g/cm³ range. The grade is specified where elevated environmental stress cracking resistance, high melt strength, and thick-wall integrity are required. The applications below are limited to established HDPE blow moulding and extrusion routes where the viscosity envelope of KM660W is appropriate; thin-wall film and high-flow injection moulding are outside the reliable processing window.
In automotive fuel tank manufacturing, KM660W is processed as the outer and inner HDPE layers of a six-layer coextruded wall. The layer sequence is outer HDPE / adhesive / EVOH / adhesive / regrind HDPE / inner HDPE, with KM660W-derived outer and inner skins totalling 58–65 wt% of the wall mass. The EVOH oxygen and hydrocarbon barrier layer is maintained at 1.5–3.0 wt%, maleic anhydride-grafted tie layers at 1.0–2.0 wt%, and the buried regrind layer at 25–35 wt%. Regrind is generated from trim flash and rejected tanks after shredding, remelting, and filtration through a 60–80 mesh screen pack. The KM660W addition ratio in the outer and inner skin layers is 100 wt% virgin resin; regrind is excluded from the exposed surfaces to preserve weld-line integrity and hydrocarbon permeation resistance.
Compliance is evaluated under UN ECE R34 Annex 5 for fire resistance, FMVSS 301 for fuel system integrity, and evaporative emission limits under EPA 40 CFR Part 86.1811 and CARB LEV III. On production-scale accumulator blow-moulding machines with 25–45 L shot volume and 1,200–2,000 kN clamp force, the HDPE melt temperature is held at 210–230 °C, while the EVOH melt is processed within 200–225 °C to avoid excessive barrier-layer degradation. Barrel residence time is limited to ≤ 15 min to limit gel formation. Parison wall-thickness programming uses axial die-gap control and radial profiling to compensate for sag; mould temperature is maintained at 15–20 °C. The terminal products are automotive fuel tanks for passenger cars and light commercial vehicles. Published KM660W-specific permeation coefficients for ethanol-containing fuel blends are limited; converter validation typically includes ASTM D638-14 tensile and ISO 179-1:2010 Charpy impact testing.
The 1,000-L composite IBC inner bottle is a single-layer extrusion blow-moulded receptacle that must withstand top-lift handling, stacking, and drop impact while containing aggressive liquid chemicals. KM660W is used at 100 wt% virgin in the product-contact wall for acids and oxidizers. For non-oxidizing general chemicals, clean in-house regrind up to 25 wt% is blended into the outer side only if the bottle passes the full UN IBC drop and leakproofness test sequence. The governing framework is UN Model Regulations Chapter 6.5, with IBC marking code 31HA1/Y. Qualification drop heights are 1.8 m, 1.2 m, or 0.8 m depending on packing group. Batch-to-batch variance in ESCR becomes significant when regrind fraction exceeds 15 wt%; each lot must be qualified by ASTM D1693 Condition C.
Production uses long-stroke accumulator blow-moulding machines with 30–50 kg shot capacity, extruder L/D 24:1–30:1, melt temperature 200–225 °C, and blow air pressure 0.6–0.8 MPa. Cycle time for a 14–18 kg bottle typically falls between 10 and 18 min because cooling is governed by the pinch-off weld. Mould water temperature is maintained at 12–18 °C. After deflashing, the top opening is CNC-trimmed and the outer surface is inspected for wall thickness distribution; the chime area is measured at a minimum 4–6 mm. Terminal products are 1,000-L IBC inner bottles for hazardous and non-hazardous chemical transport. Published data for KM660W-specific ESCR after 25 wt% regrind is limited, so qualification must be performed on production-scale bottles rather than laboratory plaques.
Tight-head and open-head drums from 30 L to 220 L are produced from KM660W on single-station accumulator blow-moulding machines. The base formulation uses KM660W at 100 wt% virgin, except where a colour masterbatch or internal regrind is permitted. Regrind from flash and rejected drums is added up to 20 wt% only if the blend meets the ESCR threshold of 1,000 h in ASTM D1693 Condition C and maintains tensile properties under ASTM D638-14. Higher regrind levels reduce the drop-test margin at the chime and pinch-off weld because the low-molecular-weight fraction from thermal history shifts the relaxation spectrum.
For dangerous goods, drums are marked UN 1H1/X1.6/250 for tight-head or UN 1H2/Y1.9/250 for open-head, with drop height, stacking load, and hydraulic pressure tests conducted under UN Model Regulations Chapter 6.1. Melt temperature is 190–220 °C, die head temperature 200–215 °C, accumulator shot weight 10–30 kg, blow pressure 0.6–0.9 MPa, and mould temperature 10–20 °C. Parison programming uses axial wall-thickness control with 80–120 programmed points to distribute material around chime and handle sections. The terminal products are 30–220 L tight-head and open-head drums and jerricans for industrial chemicals, solvents, and lubricants. Localized thinning at the pinch-off weld is the primary failure mode when mould cooling is below 10 °C or regrind content exceeds 20 wt%.
Underground fibre-optic conduit extrusion with KM660W employs a 60–90 mm single-screw extruder with L/D 30:1, a grooved feed section, and a spiral mandrel die, followed by vacuum calibration at 0.06–0.09 MPa for outside-diameter and wall-thickness control. The dry blend is composed of 97.5–98.0 wt% KM660W and 2.0–2.5 wt% carbon black masterbatch, yielding a final carbon black content of 2.0–2.5 wt% as determined by ASTM D1603-14. This addition ratio is a threshold value: below 2.0 wt% carbon black, outdoor ultraviolet weathering under ASTM G154 cycle 1 reduces notched impact retention below accepted engineering specifications; above 2.5 wt%, melt viscosity and surface roughness increase without proportional weather-resistance gain. Undispersed carbon black particles greater than roughly 10 μm can initiate melt fracture and surface pitting.
Compliance is assessed against ASTM F2160 for solid-wall high-density polyethylene conduit, ASTM D3350 for cell classification, and UL 651A for continuous-length HDPE conduit. Processing temperatures are set at 180–200 °C in the rear barrel zone, 200–220 °C in the front zone, and 210–225 °C at the die; melt temperature at the die exit is held below 230 °C. Cooling water is staged at 15–25 °C, and puller speed is adjusted to maintain 2–5% shrink-back. The terminal product is solid-wall and corrugated HDPE conduit for fibre-optic, telecommunications, and low-voltage power cable protection.
Stationary above-ground tanks for domestic heating oil, kerosene, and diesel are blow moulded from KM660W at 100 wt% virgin resin, with 2.0–3.0 wt% UV stabilizer masterbatch where the tank is installed outdoors without additional shelter. In-house regrind up to 15 wt% is permitted in non-critical sections, but not in the tank base or threaded boss areas, where ESCR and weld-line strength are limiting. The governing product standard is EN 13341 for static thermoplastic tanks for above-ground storage of domestic heating oils, kerosene and diesel fuels. ESCR is evaluated under ASTM D1693 Condition C, and impact resistance under ISO 179-1:2010.
Production is performed on large accumulator blow-moulding machines with shot capacity 15–40 kg, melt temperature 200–220 °C, mould temperature 10–18 °C, and blow air pressure 0.6–0.8 MPa. Threaded inserts are placed in the mould before closing; insert temperature is kept at 20–40 °C to reduce localized shrinkage. The terminal products are 500–5,000 L heating oil and agricultural diesel stationary tanks. The critical failure mode in service is slow crack growth at the base corners under static hydrostatic pressure; base corner wall thickness at 5,000 L scale is maintained at a minimum 7 mm. Published KM660W-specific slow crack growth data under actual tank geometries is limited.
Agricultural chemical packaging for pesticides, herbicides, and surfactants is produced from KM660W in 1–20 L monolayer blow-moulded containers. The contact layer uses 100 wt% virgin KM660W; dry colour masterbatch may be added at 0–2 wt%, but post-consumer regrind is excluded because UN certification and compatibility testing are batch-specific. Where solvent-containing formulations require lower permeation, surface fluorination is applied after moulding; this is not a resin addition and does not alter the KM660W addition ratio. Compatibility is assessed by ASTM D543-21, and post-exposure ESCR is measured under ASTM D1693 Condition C.
Packaging for dangerous goods is marked and tested under UN Model Regulations Chapter 6.1. Production uses reciprocating or shuttle blow-moulding machines with 50–80 mm extruder diameter, melt temperature 190–215 °C, blow pressure 0.5–0.7 MPa, and mould cooling 12–20 °C. The terminal products are 1–20 L HDPE containers for crop protection, adjuvants, and specialty agricultural chemicals. The main processing constraint is stress cracking accelerated by non-ionic surfactants; containers with bottom chime wall thickness below 1.2 mm may exhibit premature environmental cracking. Published KM660W-specific compatibility with individual active ingredients is limited; chemical compatibility must be tested with the actual formulation at the intended concentration and storage temperature.
Competitive TPC (Japan) HDPE KM660W prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
TPC (Japan) HDPE KM660W is an ethylene homopolymer grade supplied as white/off-white pellets and classified as a high-density polyethylene with a high-molecular-weight fraction and a broadened molecular weight distribution. The grade designation KM660W appears in supplier documentation primarily as a high-melt-strength material for heavy-duty film, large-part blow moulding, and thick-walled extrusion where the low melt mass-flow rate at 2.16 kg load restricts injection-type flow but high-load melt flow at 21.6 kg remains sufficient for extrusion. Publicly available datasheets outside Japan are condensed and do not always include complete lot-specific property tables; the numerical ranges in this document are class-representative values for high-molecular-weight HDPE of this architecture and should be verified against the supplier certificate of analysis before tooling or process validation.
Representative values for KM660W are: density 0.952–0.956 g/cm³ by ISO 1183-1:2019; melt mass-flow rate at 190 °C and 2.16 kg 0.03–0.07 g/10 min; high-load melt index at 21.6 kg 6.0–9.0 g/10 min; flow rate ratio 150–220; tensile yield 27–30 MPa; elongation at break greater than 600 %; flexural modulus 1150–1350 MPa; notched Charpy impact at 23 °C greater than 20 kJ/m²; and environmental stress-crack resistance expressed as F50 greater than 600 h by ASTM D1693-21 Condition B. These values position the material in the high-molecular-weight HDPE class rather than in the low-viscosity injection moulding or standard unimodal blow moulding classes.
The primary distinction is rheological rather than simply density-based. Standard low-MFI injection HDPE grades flow at 20–50 g/10 min under 2.16 kg, allowing thin-wall mould filling but reducing melt strength and environmental stress-crack resistance. KM660W, by contrast, exhibits a 2.16 kg melt mass-flow rate below 0.1 g/10 min while retaining a practical high-load melt index of 6.0–9.0 g/10 min at 21.6 kg. The resulting flow rate ratio of 150–220 indicates pronounced shear thinning. In converting operations, this means the material remains highly viscous at low deformation rates, which supports bubble and parison stability, but flows more readily in extruder head channels where shear rates are higher.
Compared with bimodal pipe-plant HDPE, KM660W has a different performance objective. Pipe grades are optimized for long-term hydrostatic strength, slow crack growth resistance, and stiffness over 50-year service life. They often have density above 0.958 g/cm³ and are processed at high extruder throughput. KM660W is not specified as a pipe pressure-rating material; its modulus and density are slightly lower, and its melt architecture is directed toward controlled sag, melt fracture resistance, and surface quality in blow moulding and film. The distinction matters when selecting grades for structural pipe applications, where KM660W would not replace a certified PE 100 or PE 80 resin without full hydrostatic design validation.
| Property | Test method | KM660W class-representative range | Unimodal HDPE blow moulding reference | Low-MFI injection HDPE reference |
|---|---|---|---|---|
| Melt mass-flow rate at 190 °C/2.16 kg | ISO 1133-1:2022 | 0.03–0.07 g/10 min | 0.20–0.50 g/10 min | 20–50 g/10 min |
| High-load melt index at 190 °C/21.6 kg | ISO 1133-1:2022 | 6.0–9.0 g/10 min | 3.0–5.0 g/10 min | Not usually specified |
| Flow rate ratio | Calculated | 150–220 | 80–110 | 20–40 |
| Density | ISO 1183-1:2019 | 0.952–0.956 g/cm³ | 0.952–0.960 g/cm³ | 0.955–0.965 g/cm³ |
| Tensile yield stress | ISO 527-2:2012 | 27–30 MPa | 26–29 MPa | 28–32 MPa |
| Flexural modulus | ISO 178:2019 | 1150–1350 MPa | 1100–1300 MPa | 1200–1500 MPa |
| ESCR F50 | ASTM D1693-21 Condition B | >600 h | 100–300 h | 5–20 h |
| Vicat softening A50 | ISO 306:2022 | 124–128 °C | 123–127 °C | 126–130 °C |
Values in the middle three columns are class-representative envelopes from published resin databases for high-molecular-weight HDPE, standard unimodal blow moulding HDPE, and low-viscosity injection HDPE. They are not guaranteed minima or maxima. For tooling design and process capability studies, the supplier certificate of analysis and lot-specific rheology data should be used.
The melt flow characterization of KM660W follows ISO 1133-1:2022 using a preheated die and timed extrudate collection. Because the 2.16 kg value falls below 0.1 g/10 min, the measurement is sensitive to die cleanliness, melt temperature uniformity, and piston-tip leakage. The 21.6 kg high-load method is more repeatable and is the preferred quality-control parameter. A flow rate ratio above 150 is associated with broadened molecular weight distribution. This broadening reduces the sharpness of the transition from solid-like to liquid-like melt behavior, which has practical consequences in extruder head pressure control and die swell management.
Density is measured by ISO 1183-1:2019 on compression-moulded plaques conditioned according to ISO 291:2008. The 0.952–0.956 g/cm³ range is typical for HDPE grades designed for high stress-crack resistance. Higher density would increase stiffness but usually lowers ESCR and impact properties. Tensile yield stress values of 27–30 MPa by ISO 527-2:2012 and flexural modulus values of 1150–1350 MPa by ISO 178:2019 reflect the balance between stiffness and ductility. Elongation at break above 600 % is characteristic of a properly stabilized homopolymer with a low concentration of large oxidized gel defects, although film or moulded-part performance also depends on process-induced orientation.
Environmental stress-crack resistance is a critical differentiator for KM660W in service conditions involving detergents, alcohols, oils, or weak acids. The ASTM D1693-21 bent-strip test, Condition B, with 100 % Igepal CO-630 at 50 °C, gives F50 values above 600 h for class-representative formulations. This level significantly exceeds standard unimodal blow moulding HDPE, which commonly fails between 100 h and 300 h under the same condition. The improvement arises from the high-molecular-weight fraction and the concentration of tie molecules between crystalline lamellae, not from density alone. Flow-induced orientation in the wall of a large blow-moulded container or in a thin film can further improve resistance to slow crack propagation but also creates residual stress that must be managed through tooling geometry and cooling rate.
Accumulator-head blow moulding of large containers, industrial drums, and complex technical parts places a specific demand on low-shear melt strength. The parison is extruded, cut, transferred, and inflated under gravity before mould closing. During this interval, the melt deformation rate is relatively low, and sag resistance is governed by high-molecular-weight chains and long relaxation times. KM660W is formulated to provide greater parison hang time than a standard unimodal HDPE of similar density. On production-scale accumulator-head machines with clamp force in the 100–300 ton range, parison swell is reported to be higher than for conventional blow moulding grades, often requiring die gap adjustment of 10–20 % to maintain target wall thickness.
Melt temperature at the die is normally controlled between 190 °C and 210 °C. Below 185 °C, head pressure increases and surface melt fracture may appear as shark-skin on thicker sections. Above 220 °C, sag resistance declines and cycle time increases because of additional heat load. Mould temperature is typically maintained between 10 °C and 30 °C to achieve adequate cooling without excessive condensation in humid plants. Blow pressure is generally 0.6–0.9 MPa, depending on part size and wall thickness. The broadened molecular weight distribution reduces the tendency for variable wall thickness at the pinch-off, but pinch-off geometry, flash thickness, and mould venting remain critical to production consistency.
The high ESCR of KM660W is particularly relevant for blow-moulded containers holding aggressive liquids, including industrial detergents, surfactant-based cleaners, and agricultural auxiliary chemicals. Stress concentrations at the pinch-off and sharp radii are the dominant initiation sites for environmental stress cracking. In those regions, orientation can reduce ESCR unless the tooling is designed to avoid abrupt thickness transitions. A minimum radius of 3 mm at internal corners is often used for large HDPE containers, although the specific value depends on part volume, wall thickness, and service loading.
Where KM660W is directed to high-strength blown film, the same high-molecular-weight architecture changes bubble cooling economics. Blow-up ratios of 3:1 to 5:1 and die gaps of 1.2–2.0 mm are typical for high-molecular-weight HDPE film. The high melt strength permits a taller neck height and improved bubble stability at thin gauges below 25 µm. Die temperatures are held between 190 °C and 210 °C, with frost line height usually set from 6 to 10 die diameters. Increasing frost line height beyond 12 die diameters may destabilize the bubble and reduce gauge uniformity. Film toughness is influenced by tear orientation, with machine-direction and transverse-direction tear strength both affected by blow-up ratio, neck height, and frost line position.
HDPE is not classified as hygroscopic, so KM660W does not generally require pre-drying. However, when pellets are transferred from cold silos into a warm plant with relative humidity above 60 %, surface condensation can introduce moisture. In such conditions, pre-drying at 80 °C for 2–3 h is recommended. Drying above 90 °C can cause pellet tackiness and bridging in the hopper because the polymer approaches its Vicat softening range.
The processing window for KM660W should not exceed 230 °C for extended residence time. Residual oxygen, metal oxides, and shear heating in the melt promote thermo-oxidative degradation above this threshold. Excursions above 260 °C accelerate chain scission, causing a detectable drop in melt viscosity, gel formation, discoloration, and odour. Dead spots in the die head, poorly streamlined adapters, and extended residence beyond 5 min at high temperature are common failure sources. Oxidative induction time testing by ASTM D3895 at 200 °C on stabilized HDPE can be used as a quality-control indicator, but the value is formulation-specific and not a direct predictor of processing stability in high-shear equipment.
Natural versions of KM660W contain a phenolic/phosphite antioxidant package and are not intended for long-term outdoor exposure unless a UV-stabilized or carbon black-containing version is specified. For black grades, carbon black content in the range of 2.0–2.5 wt% is typical for weathering resistance, but dispersion quality must be monitored because poor carbon black dispersion can lower strain-at-break and create film defects. Storage should be in a dry, ventilated area below 40 °C, away from direct sunlight, strong oxidizers, aromatic solvents, and chlorinated hydrocarbons. Contamination with low-molecular-weight alcohols or ester-based release agents can accelerate environmental stress cracking in formed parts.
| Regulatory area | Reference standard or regulation | Typical requirement | KM660W note |
|---|---|---|---|
| European food contact | Regulation (EU) No 10/2011 | Overall migration limit 10 mg/dm² | Compliance must be confirmed on the finished article; resin compliance alone is not sufficient. |
| United States food contact | FDA 21 CFR 177.1520 | Olefin polymers; use conditions and extractives limits | Supplier food-contact statement required before use. |
| Hazardous substances in electrical equipment | Directive 2011/65/EU RoHS | No intentionally added Pb, Cd, Hg, Cr(VI), PBB, PBDE | Requires supplier SDS and analytical proof; compound-specific. |
| REACH authorization | Regulation (EC) No 1907/2006 | No SVHC above 0.1 % w/w if declared | Verify via supplier safety data sheet and declaration. |
Sourcing specifications for KM660W should require the supplier to report melt flow rate, density, ESCR, tensile yield, flexural modulus, and stabilizer package on each lot. Batch-to-batch variance of high-molecular-weight ethylene copolymerization can shift high-load melt index by more than 0.5 g/10 min. This shift is sufficient to alter parison hang time in large-part blow moulding and neck height in blown film. Process validation studies should therefore use a defined rheology window rather than a single nominal value. Tooling trials should include at least two lots representing the upper and lower melt flow bounds of the purchase specification.
KM660W should not be blended indiscriminately with low-viscosity injection HDPE or regrind from unrelated processes. Blending reduces the high-molecular-weight fraction, lowers ESCR, and steepens the parison sag response. If regrind is used, it should be clean, dry, and limited to the same grade family. The addition of more than 20 % mixed-source regrind can produce measurable shifts in high-load melt index, die swell, and environmental stress-crack resistance, depending on the source material. Processors should also avoid acid-functional additive packages, certain metal stearates, and some amine-based stabilizers that can interact with the base antioxidant system; compatibility should be confirmed by melt-flow stability, colour, and gel studies before plant-scale use.