Tpc Japan Hdpe Kl370c

TPC (Japan) HDPE KL370C

    • Product Name: TPC (Japan) HDPE KL370C
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 467046
    Density 0.957 g/cm³
    Melt Flow Rate 0.35 g/10 min
    Tensile Strength At Yield 29 MPa
    Tensile Elongation At Break 800%
    Flexural Modulus 1.2 GPa
    Vicat Softening Point 128 °C
    Melting Point 135 °C
    Brittleness Temperature < -70 °C
    Hardness Shore D 65
    Environmental Stress Crack Resistance >1000 h
    Mold Shrinkage 0.02 cm/cm
    Thermal Conductivity 0.5 W/m·K
    Specific Heat Capacity 1.9 J/g·°C
    Coefficient Of Linear Thermal Expansion 1.2E-4 cm/cm/°C
    Dielectric Constant 2.3
    Volume Resistivity 1E17 ohm·cm
    Water Absorption 0.01%

    As an accredited TPC (Japan) HDPE KL370C factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Packaging: TPC (Japan) HDPE KL370C comes in 25 kg multilayer paper bags, palletized and stretch-wrapped for shipping.
    Container Loading (20′ FCL) 20′ FCL container loading of TPC (Japan) HDPE KL370C in 25 kg bags, palletized, securely stowed for ocean export.
    Shipping TPC (Japan) HDPE KL370C is a non-hazardous high-density polyethylene resin. Ship in sealed 25 kg bags or bulk containers, kept dry and away from heat, sparks, and oxidizing agents. Not regulated as dangerous goods under DOT, IMDG, IATA, or ADR; standard freight handling applies.
    Storage Store TPC (Japan) HDPE KL370C in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and oxidizing agents. Keep original bags or containers tightly closed, palletized, and off the floor to prevent moisture and contamination. Avoid prolonged UV exposure and static buildup. Maintain clean handling areas; protect from physical damage and follow local regulations and manufacturer’s safety data sheet.
    Shelf Life Shelf life is typically 24 months if stored in original unopened packaging under cool, dry conditions away from sunlight.
    Application of TPC (Japan) HDPE KL370C

    For the blow moulding of UN-certified open-head drums and tight-head jerricans, TPC (Japan) HDPE KL370C is processed on an accumulator-head extrusion blow moulding line with barrel zone setpoints between 180°C and 210°C, the die head held 5–10°C below the rear zone to increase melt strength and stabilise parison hang. The formulation addition ratio is typically 96.5–98.0 wt% KL370C, 2.0–2.5 wt% carbon black masterbatch of 50% carbon black loading, 0.05–0.10 wt% hindered phenolic antioxidant, and 0.05–0.10 wt% calcium stearate acid scavenger. The downstream production process uses parison programming with 30-point axial wall thickness control; in the 220 L open-head drum body, wall thickness is maintained between 1.8 mm and 2.6 mm, while the pinch-off zone must cool below 80°C before demoulding to avoid weld-line splitting. The terminal products are 220 L open-head drums compliant with UN 1H2/Y, and 5–30 L tight-head jerricans compliant with UN 3H1/Y; containers are tested under 49 CFR Part 178.603 and ADR/RID Chapter 6.1, with packaging group II liquids requiring no rupture after a 1.2 m drop at -18°C. At mould temperatures below 8°C or relative humidity above 70%, condensation on the mould surface can generate pitting; when changing from a carbon black formulation to an unpigmented food-contact batch, the accumulator head must be purged with nitrogen to prevent gel contamination.

    What Controls Parison Sag in Six-Layer HDPE Fuel Tank Coextrusion?

    Parison sag on a six-layer coextrusion line equipped with six 25:1 L/D extruders feeding a spiral mandrel die is governed by the apparent melt viscosity of KL370C under low-shear sag conditions; processors typically maintain the high-load melt flow index at 21.6 kg and 190°C within the datasheet range and measure sag length at a fixed drop time of 20–40 s on accumulator heads with clamp force between 3,500 kN and 5,000 kN. The formulation addition ratio is expressed as layer mass distribution rather than masterbatch let-down: HDPE outer skin 35–40 wt%, regrind layer 30–40 wt%, maleic anhydride-grafted PE tie layer 1.5–2.5 wt%, EVOH barrier 1.5–3.0 wt%, second tie layer 1.5–2.5 wt%, and HDPE inner skin 20–25 wt%. In the regrind layer, KL370C is blended with up to 20 wt% post-industrial fuel tank trim, while the outer and inner skins are produced from 100% virgin KL370C. The downstream coextrusion process must hold EVOH at 195–215°C and purge at shutdown to avoid thermal degradation; a 10°C overshoot above the EVOH upper limit will generate black specks and odour. Compliance is anchored to UN ECE R34.03 Annex 4 fire resistance and Annex 5 impact, plus ASTM D638-14 for tensile yield not less than 20 MPa and ASTM D790-17 for flexural modulus characterisation. Blow moulds are textured with 25–50 µm depth venting grooves to prevent air entrapment, and pinch-off flash is recycled only after two passes through a 100 µm screen changer. The terminal products are 45–80 L coextruded fuel tanks for passenger vehicles and off-road equipment. Published data for KL370C in cyclic CNG fuel tank service is limited, and the grade is not specified for contact with fuel blends exceeding 10 vol% alcohol without barrier validation.

    Where composite IBC liners are produced for chemical distribution, KL370C is blow moulded into 1,000 L inner bottles on a high-output accumulator machine with a 120 mm screw diameter, 30:1 L/D, and a 125 kg melt reservoir. The formulation addition ratio for the IBC liner is 97.7–99.0 wt% KL370C, 0.05–0.10 wt% hindered phenolic antioxidant, 0.02–0.05 wt% phosphite process stabiliser, and 2.0–2.5 wt% carbon black masterbatch where UV exposure during outdoor storage is anticipated; unpigmented liners for food contact omit carbon black and rely on 0.15–0.25 wt% HALS. Downstream, the bottle is cooled in a temperature-controlled fixture at 20–25°C to maintain wall thickness at the top and bottom chimes of 2.0–3.0 mm and sidewall of 1.5–2.0 mm; chime-radius thinning below 1.5 mm can reduce top-load resistance below the 8,000 N value commonly specified by buyers for 3-high rail shipment. The terminal product is the inner receptacle of a UN 31HA1/Y composite IBC, tested under ADR/RID Chapter 6.5 for leakproofness at 20 kPa air pressure and hydraulic pressure at 100 kPa for 10 minutes. Accumulator-head machines running KL370C at 190–200°C exhibit a drop in parison hang strength if melt temperature exceeds 210°C, causing bottom-thinning beyond the 2.0 mm minimum in heavier-wall designs.

    If Fluorination Is Specified for Solvent Barrier Performance

    Post-mould fluorination of KL370C containers using a 1.0–2.5 vol% fluorine-in-nitrogen mixture at 40–60°C for 10–30 minutes reduces permeation of xylene and aromatic solvents by converting surface polyethylene to a fluoropolymer barrier less than 0.5 µm thick. For agrochemical sprayer tanks and 10–25 L narrow-mouth jugs, the bulk formulation addition ratio is 96.0–97.5 wt% KL370C, 2.0–2.5 wt% carbon black masterbatch, 0.15–0.30 wt% HALS UV stabiliser, 0.05–0.10 wt% antioxidant, and 0.05–0.10 wt% calcium stearate; amine-based antistatic agents are excluded because amine functionality can retard surface fluorination by competing for reactive sites. Downstream production uses a two-station shuttle blow moulding machine with parison programming and a fluorine barrier treatment line. The terminal product is a fluorinated UN 3H1/Y or UN 3H2/Y container; compliance includes ASTM D1998-21 for moulded tank design stress and 49 CFR Part 178.603 drop testing at -18°C with a 1.2 m drop height. The fluorination process must be followed by a 30-minute post-treatment purge with nitrogen to remove residual fluorine before unloading; operators must verify surface fluorine-to-carbon ratio by X-ray photoelectron spectroscopy at 1.0–1.5 rather than relying on post-hoc permeation tests. For tanks holding aqueous formulations with pH below 3.0, published field data indicates surface fluorination may reduce stress cracking but does not replace chemical resistance validation.

    Marine Buoyancy Structures and Low-Temperature Impact Response

    Marine buoyancy shells blown from KL370C require an extrusion blow moulding line with a 90 mm screw, 25:1 L/D, and a 40 kg accumulator head to maintain a parison drop length of 2.5–3.0 m without sag-induced bottom thinning. The formulation addition ratio for marine fenders and mooring buoys is 96.5–97.5 wt% KL370C, 2.0–2.5 wt% carbon black masterbatch with 50% carbon black content, 0.30–0.45 wt% hindered amine light stabiliser, 0.05–0.10 wt% phosphite antioxidant, and 0.02–0.05 wt% processing aid. The terminal products are cylindrical buoyancy modules, dock fenders, and channel marker floats produced in wall thicknesses of 4–12 mm. Compliance for UV exposure is assessed under ISO 4892-3:2016 with a 2,000 h exposure cycle and a ΔE target below 4.0, while low-temperature impact verification follows ASTM D1998-21 at -20°C; marine-specific certification is not universal and is often buyer-specified. The process risk is cooling-time-induced shrinkage: wall thickness above 10 mm may require 15–25 minutes of in-mould cooling at 15–20°C mould water temperature to limit volumetric shrinkage below 2.5% and to avoid sink marks at stiffener intersections. Adding more than 0.45 wt% HALS in unpigmented marine service can exude to the surface at mould temperatures above 20°C, causing visible bloom and potential solvent wipe failure.

    When sheet gauge exceeds 8 mm, extrusion of KL370C into 8–25 mm thick sheet for thermoformed pallets and separator dunnage uses a 120 mm single-screw extruder with a barrier screw and melt pump, running at 190–210°C, then passes through a three-roll stack with roll temperatures of 30–60°C. The formulation addition ratio for sheet is 99.5–99.8 wt% KL370C, 0.03–0.08 wt% hindered phenolic antioxidant, 0.02–0.05 wt% phosphite process stabiliser, and 0.02–0.05 wt% external lubricant; carbon black is not added unless electrostatic discharge protection is specified for electronics dunnage. Thermoforming is conducted on twin-sheet equipment at a sheet surface temperature of 165–175°C, with plug depth set to avoid thinning below 20% of the original sheet gauge in the corner radii. The terminal products are twin-sheet pallets, separator sheets, and dunnage trays used in automated warehousing. Compliance for pallet load capacity is tested under ISO 8611-1:2011, while tensile elongation at yield is measured to ASTM D638-14; material in dunnage service is not specified for direct food contact unless separately cleared under FDA 21 CFR 177.1520. At sheet thickness above 25 mm, published process data is limited, and cooling capacity rather than extruder output becomes the controlling limitation.

    Blow Moulding Double-Wall Panels for Outdoor Storage and Enclosures

    Double-wall outdoor enclosure panels produced from KL370C are blow moulded on a single-station machine with a 100 mm extruder, 24:1 L/D, and a 75 kg shot accumulator; the mould closing speed is set below 300 mm/s to avoid tearing the parison when pinch-off area exceeds 1,200 cm². The formulation addition ratio for UV-stabilised outdoor panels is 97.2–98.0 wt% KL370C, 0.20–0.30 wt% HALS, 0.05–0.10 wt% antioxidant, 1.0–2.0 wt% pigment masterbatch or 2.0–2.5 wt% carbon black masterbatch, and 0.02 wt% processing aid. The terminal products are door panels, shed wall panels, and enclosure panels with 20–40 mm double-wall cross-sections. Compliance for weathering and mechanical properties follows ISO 4892-2:2013 for xenon-arc exposure and ASTM D790-17 for flexural creep; structural panel assemblies are not regulated under a single global standard and are tested to customer-defined load cases. At the transition from the solid pinch-off weld to the hollow double-wall section, low mould temperature and excessive clamping speed are known failure sites, and Charpy impact strength must be verified according to ISO 179-1:2010 at -30°C. Post-mould fixturing for 24–48 h is required to stabilise panel bow to below 3 mm per 1,000 mm span before assembly.

    Water Storage Vessels and the NSF/ANSI/CAN 61 Extraction Boundary

    In potable water service, vertical storage tanks produced from KL370C are blow moulded as single-piece shells with wall thickness 6–15 mm and capacities of 500–10,000 L, using an accumulator-head machine with a 120 mm screw and 40:1 L/D to maintain homogeneous melt at 185–200°C. The formulation addition ratio for potable-water contact is 99.7–99.9 wt% KL370C, 0.05–0.10 wt% hindered phenolic antioxidant, and 0.02–0.05 wt% phosphite process stabiliser; carbon black and HALS are omitted unless the unit is designated for outdoor non-potable water storage, in which case 2.0–2.5 wt% carbon black and 0.25–0.35 wt% HALS are charged. The terminal products are cylindrical vertical storage tanks and conical-bottom dosing tanks for water treatment plants. Compliance is established through NSF/ANSI/CAN 61 by the terminal fabricator, not by the resin supplier, because extraction test results depend on the moulded surface-to-volume ratio and post-mould cleaning; EU drinking water compliance is assessed under Directive (EU) 2020/2184 and national migration limits. The process must avoid zinc stearate in the additive package because zinc-containing residues can elevate extraction test metals above detectable thresholds. A resin moisture content above 0.03% can produce surface splay at the vented mould surface; published data for KL370C at wall thickness above 15 mm is limited.

    Free Quote

    Competitive TPC (Japan) HDPE KL370C prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    The high-density polyethylene grade designated KL370C, supplied by TPC (Japan), is classified primarily as an extrusion blow-moulding resin for rigid packaging and industrial containers. Representative property data reported in distributor datasheets place nominal density at 0.957 g/cm³ when conditioned at 23 °C under ASTM D1505 or ISO 1183-1:2019, and high-load melt index measured at 190 °C/21.6 kg in the range of 6.0–7.5 g/10 min per ISO 1133-1:2022. The low-load melt index at 190 °C/2.16 kg is correspondingly low, typically 0.25–0.40 g/10 min, which indicates a high-molecular-weight structure selected for parison melt strength rather than high-speed injection flow. The grade is differentiated from general-purpose HDPE by its stress-crack resistance and stiffness retention in thick-walled containers for household chemicals, lubricants, and agricultural adjuvants where environmental stress-cracking is a documented field failure mode. Because published lot-specific certification data for this exact configuration remain limited in public repositories, the numerical values in this overview should be interpreted as representative grade-band values rather than guaranteed minimums unless stated in a supplier certificate of analysis.

    PropertyStandard / conditionRepresentative value
    DensityISO 1183-1:2019, 23 °C0.956–0.958 g/cm³
    High-load melt indexISO 1133-1:2022, 190 °C/21.6 kg6.0–7.5 g/10 min
    Melt flow rateISO 1133-1:2022, 190 °C/2.16 kg0.25–0.40 g/10 min
    Tensile stress at yieldASTM D638-14, 50 mm/min27–29 MPa
    Tensile elongation at breakASTM D638-14>600%
    Flexural modulusISO 178:20191050–1250 MPa
    Notched Izod impact, 23 °CISO 180:202310–14 kJ/m² or non-break
    ESCR F50ASTM D1693-15b, Condition B, 100% Igepal CO-630≥300 h
    Vicat softening pointISO 306:2022 A50123–128 °C
    Heat deflection temperatureASTM D648-18, 0.455 MPa68–76 °C

    The tabulated values are not a substitute for lot-specific certification data. Property ranges reflect distributor literature and standard-grade envelopes for high-molecular-weight blow-moulding HDPE in this density and high-load melt index band.

    What separates KL370C from injection-moulding and film-extrusion grades within the same supplier portfolio?

    The most immediate difference is rheological. Injection-moulding HDPE grades are routinely specified by melt flow rate at 190 °C/2.16 kg of 5–20 g/10 min, whereas KL370C is specified by high-load melt index at 21.6 kg because the lower load does not generate sufficient mass-flow signal for reliable lot control. Film-extrusion HDPE grades in the same density range are often tuned for low draw resonance and bubble stability; this requires narrower molecular-weight distribution and lower melt swell than is acceptable in an intermittent blow-moulding melt. KL370C is positioned in the higher-viscosity, higher-swell segment of the portfolio, which permits a hanging parison to retain wall-thickness uniformity over drop lengths up to roughly 400 mm in production trials, although exact sag resistance depends on melt temperature and die tooling.

    Compared with a typical injection-moulding grade of density 0.958 g/cm³, KL370C exhibits lower melt flow and higher notched impact strength, but it is not a drop-in injection-moulding substitute because its high viscosity can produce gate-cold-slug inhibition and unacceptable cycle-time loss in thin-wall cold-runner moulds. Compared with clarified random copolymer polypropylene used for some rigid packaging, HDPE KL370C is translucent to opaque in thick sections, has lower heat-distortion temperature, but demonstrates superior environmental stress-crack resistance in contact with polar liquids and surfactants. The material is specified where opacity, chemical compatibility, and pinch-off weld integrity carry greater weight than contact clarity or low-temperature packaging aesthetics.

    Across a single-station shuttle blow-moulding line with a 65 mm, 24:1 L/D grooved-barrel extruder, the material is normally processed at a rear-to-die temperature profile of 170–210 °C and a melt temperature of 185–200 °C. Lower melt temperatures below 175 °C increase die-head pressure and may produce sharkskin melt fracture at the parison free surface, whereas temperatures above 220 °C can cause excessive parison sag and a measurable reduction in wall-thickness control. The practical melt-temperature window is therefore narrow enough that a change of less than 10 °C can shift parison length and die swell on small tooling; production trials should map temperature before a new die is fixed. Blow pressure is typically 0.6–0.8 MPa; mould temperature is held between 10 °C and 30 °C for cycle-time management, but higher mould temperatures improve weld-line healing at the pinch-off and reduce frozen-in stress in thick bases.

    Drying is not normally required for KL370C when packaging remains sealed. If the resin is stored at relative humidity above 60% or exposed to condensation, surface moisture can produce porosity in parison walls and poor weld-line definition. A desiccant dryer operated at 80 °C for 2 h is sufficient for the removal of surface moisture; longer oven exposure without inert-gas purge can cause oxidation and increase gel speck formation on blow-moulded surfaces. For continuous-extrusion shuttle lines with die gap between 1.2 mm and 2.0 mm, die swell is commonly observed in the range of 35–45%; accumulator-head machines may operate with a slightly narrower die gap to maintain the same parison diameter. Weight swell and diameter swell must be separated during tooling design because the high-molecular-weight tail increases both properties in relation to a low-density polyethylene of equivalent melt index.

    Mechanical property verification is bound to ISO and ASTM test methodology, not nominal data

    Tensile, flexural, and impact values assigned to KL370C should be specified with test method and specimen conditioning. Under ASTM D638-14, the reported tensile stress at yield is typically 27–29 MPa at 50 mm/min, with elongation at break above 600%. Flexural modulus according to ISO 178:2019 is approximately 1050–1250 MPa, while notched Izod impact at 23 °C under ISO 180:2023 is generally reported as 10–14 kJ/m²; some specimens may not break, and such a result should be recorded as non-break rather than a numerical energy if the tab geometry exceeds the method’s validity limits. Environmental stress-crack resistance is measured by ASTM D1693-15b Condition B in 100% Igepal CO-630; typical values in distributor literature are ≥300 h at F50. Thermal resistance is moderate: Vicat softening temperature under ISO 306:2022 A50 is approximately 123–128 °C, and heat deflection temperature under ASTM D648-18 at 0.455 MPa is 68–76 °C. These thermal values place an upper continuous-use limit near 60–65 °C for stressed chemical containers, not at the Vicat point.

    When a container requires UN-certified dangerous-goods design, the material alone does not confer compliance

    KL370C may be used as the outer body material for UN-type packaging, but certification is assigned to the finished container under the UN Model Regulations, Chapter 6.1, including drop height, stacking load, leakproofness, and hydraulic pressure performance after test regimes relevant to the packaged substance. A resin grade cannot be certified independently. In practice, the high environmental stress-crack resistance of KL370C supports retention of hoop strength in detergent, lubricant, and agrochemical containers, but the pinch-off weld, handle geometry, wall-thickness distribution, and moulded-in stress remain failure-prone regions. Formulators and moulders should not assume that a designed container passes UN testing merely because the base resin is a high-ESCR HDPE; prototype testing at produced wall thickness and closure torque is required.

    For food-contact and pharmaceutical packaging, the as-supplied resin grade must be evaluated under the applicable national or regional positive list. HDPE may be permitted under 21 CFR 177.1520 when the finished polymer meets extractable fraction limits and the intended use is supported by migration testing, but each supplier lot should have a food-contact compliance statement rather than a generic reference to the regulation. Under Regulation (EU) No 10/2011, the base polymer and additives are subject to overall migration and specific migration limits using the correct food simulants; the presence of process aids or external lubricants can alter total migration values. For REACH, the supplier-specific SVHC candidate-list declaration under Regulation (EC) No 1907/2006 is required; a blanket statement that KL370C is SVHC-free is not acceptable without dated supplier documentation.

    Regulatory instrumentTest method / clauseApplicability to KL370C as supplied
    FDA 21 CFR 177.1520Olefin polymer criteria, extractable fraction limitsConformance depends on end-use migration testing and lot-specific supplier letter
    Regulation (EU) No 10/2011Overall migration and specific migration limits in food simulantsRequires finished-article testing; base-polymer listing alone is insufficient
    REACH (EC) No 1907/2006SVHC candidate-list declaration, Article 33Supplier-specific verification required per lot
    RoHS Directive 2011/65/EUHeavy metal thresholds: Pb 1000 ppm, Cd 100 ppm, Hg 1000 ppm, Cr(VI) 1000 ppmApplicable only if the packaged article falls within the directive scope; supplier declaration required
    UN Model Regulations, Chapter 6.1Drop, stacking, leakproofness, hydraulic pressure on finished containerResin supports but does not guarantee packaging certification

    Heat history, regrind, and weld-integrity thresholds in production

    KL370C is sensitive to repeated extrusion heat history. Regrind addition above 20–25% by weight can reduce environmental stress-crack resistance and shift the high-load melt index upward beyond acceptable control limits, especially if the regrind originates from containers with high surface contamination. If regrind use is mandatory, blending should be controlled gravimetrically and the resulting mixture should be tested for high-load melt index and ESCR under ASTM D1693-15b on the same day as processing. A measurable increase in gel speck formation on the container exterior often appears before bulk mechanical properties collapse; this should be treated as an early warning of excessive oxidative degradation.

    Pinch-off weld integrity is a primary production-control parameter. On a single-head shuttle machine, insufficient pinch compression can leave a weak base weld that fails drop testing at -18 °C even when the resin lot meets all specification limits. Pinch-off insert edges should be inspected for wear; a rounded edge produces variable weld thickness and can create a notch-like crevice at the container base interior. The weld can also be weakened by parison contaminants, especially silicone-release residues or external lubricants migrating from upstream conveying equipment. In such cases, the failure mode is typically incomplete fusion at the weld centerline, not brittle fracture of the polymer matrix.

    In agrochemical packaging, the most demanding end-use condition is frequently not ambient storage but prolonged contact with ester-based emulsifiable concentrate solvents and surfactants. Under ASTM D1693-15b Condition B, KL370C shows substantial resistance, but field experience indicates that container design stress concentrations at handle attachments and sharp base corners can initiate slow crack growth even when the coupon specimen passes. For household chemical bottles subject to overhead stack loading in high-humidity warehouses, creep of the HDPE wall at elevated summer temperatures can produce dimensional distortion; this is a design-load issue governed by modulus-temperature dependence and not a resin-defect indicator. Published data for KL370C under continuous compressive load at 40 °C and 90% relative humidity are limited; stack-hazard assessments should be conducted on the filled container rather than on the neat resin.

    Top