| HS Code | 126301 |
| Density | 0.954 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 0.30 g/10 min |
| Tensile Strength At Yield | 29 MPa |
| Tensile Elongation At Break | 500% |
| Flexural Modulus | 1200 MPa |
| Vicat Softening Temperature | 124°C |
| Heat Deflection Temperature At 0 45 Mpa | 78°C |
| Environmental Stress Crack Resistance | >1000 h |
| Shore D Hardness | 66 |
| Coefficient Of Linear Thermal Expansion | 1.2E-4 cm/cm/°C |
| Thermal Conductivity | 0.50 W/m·K |
| Specific Heat Capacity | 1.90 J/g·°C |
| Dielectric Constant | 2.30 |
| Volume Resistivity | 1E+16 Ω·cm |
| Water Absorption | 0.01% |
| Oxygen Index | 17% |
As an accredited TPC (Japan) HDPE KKZ51C factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | TPC (Japan) HDPE KKZ51C is supplied in 25 kg net paper bags, palletized, typically 40 bags (1,000 kg) per pallet. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): TPC (Japan) HDPE KKZ51C, non-hazardous 25 kg bags, palletized, stretch-wrapped, securely braced, ~20 MT net. |
| Shipping | TPC (Japan) HDPE KKZ51C is a non-hazardous polyethylene resin shipped as general cargo. Typically packed in 25 kg bags or 500–1000 kg jumbo bags, palletized and stretch-wrapped. Transport in clean, dry containers or trucks; keep away from moisture, sunlight, heat, and ignition sources. No special DG documentation required. |
| Storage | Store TPC (Japan) HDPE KKZ51C in original, tightly closed bags or containers in a cool, dry, well-ventilated warehouse. Protect from direct sunlight, moisture, heat, flames, and oxidizing agents. Keep away from strong acids, bases, and incompatible chemicals. Use clean, palletized stacks; avoid excessive stacking and UV exposure. Observe local regulations and the manufacturer’s SDS. |
| Shelf Life | Shelf life is typically two years from manufacture when stored unopened in a cool, dry, ventilated area away from direct sunlight. |
On co-rotating twin-screw compounding lines with L/D ratios between 36:1 and 44:1 and screw diameters from 50 mm to 120 mm, HDPE KKZ51C is preblended with carbon black masterbatch and stabilizer prior to entering barrel zones held between 180°C and 220°C. The recommended addition profile for gravity-flow drainage and cable-conduit compounds is 96.0–97.5 wt% KKZ51C, 2.5–3.5 wt% carbon black masterbatch at 40% carbon black loading, and 0.2–0.5 wt% antioxidant/processing stabilizer masterbatch. Compliance references for the converted product include EN 13476-2:2018 for structured-wall piping, ISO 8772:2006 for high-density polyethylene drainage pipe, ASTM D3350-21 for material classification, and ISO 4892-2:2013 xenon-arc exposure for outdoor UV stability. Downstream conversion proceeds on single-screw extruders with grooved feed sections and L/D ratios of 30:1 to 36:1, feeding pipe dies from 100 mm to 1200 mm outside diameter; corrugator block temperatures are controlled at 8–20°C, and melt temperature at the die is maintained below 230°C to suppress surface pitting and uncontrolled melt fracture. Screen packs with 40/60/80 mesh layers maintain die-head pressure between 15 MPa and 25 MPa; residence times above 90 s increase gel counts measurable as pipe inner-wall roughness. Terminal finished product types are twin-wall corrugated drainage pipes, underground cable conduits, and gravity-flow rainwater pipes.
Accumulator-head blow moulding machines of 25–50 t clamp force process KKZ51C with barrel zone settings from 185°C to 215°C, accumulator temperature 10–20°C below the die head, and die gap adjustment between 0.6 mm and 1.8 mm as container volume and wall thickness dictate. The addition ratio for opaque industrial container stock is 98.0–99.0 wt% KKZ51C, 1.0–2.0 wt% colour concentrate, and 0.05–0.20 wt% fluoropolymer-based processing aid where intermittent extrusion generates die build-up. Compliance is governed by UN 1H1/1H2 dangerous-goods packaging approvals under ADR/RID, FDA 21 CFR 177.1520(c) for olefin polymers in food contact, EU 10/2011 overall migration limits of 10 mg/dm², and ISO 1183-1:2019 density classification. In production-scale trials, parison sag exceeding 6% bottom wall-thickness reduction between the first and last shot indicates accumulator temperature creep or insufficient melt strength; pinch-off weld integrity is verified by filled-container drop tests from 1.8 m according to the applicable packaging-group protocol. On accumulator-head machines, flash weight drift of 3–7% across a 5000-cycle run is controlled by trim of the die gap and accumulator temperature; parison programming maps use 25-point wall thickness control. Terminal finished products are closed-head jerry cans of 5 L to 30 L, open-top pails, and UN-certified industrial chemical packaging.
Three-layer blown-film lines with die diameters from 1600 mm to 3500 mm and die gaps of 1.6–2.4 mm process KKZ51C-heavy skins for geomembrane and industrial liner formats. The symmetrical A-B-A formulation uses 85–95 wt% KKZ51C in each skin layer, 5–15 wt% LLDPE with melt index 0.5–1.0 g/10 min for tear balance modification, and 0.5–1.5 wt% UV stabilizer masterbatch for exposed service. Industry compliance for smooth black geomembrane is anchored to GRI GM13:2021, ASTM D5199 thickness tolerance of ±5%, ASTM D5397 hydrostatic resistance, and EU 10/2011 where the film enters food contact. Process parameters on commercial lines include extruder zones from 195°C to 215°C, blow-up ratio 2.0:1 to 3.0:1, frost-line height 700–1300 mm, internal bubble cooling air at 10–20°C, and melt pressure before the die between 25 MPa and 35 MPa. Die gaps below 1.6 mm produce elevated melt pressure and outer-lip die build-up; screen packs with 60/80 mesh layers and internal bubble cooling reduce gauge scatter. Bubble instability onset occurs below 600 mm frost-line height at high extrusion outputs; films below 0.5 mm gauge without internal bubble cooling tend to show gauge variation above ±5%. Terminal finished product types are landfill geomembranes, canal liners, and secondary containment membranes.
Multi-cavity closure lines with 2500–8000 kN clamp force and valve-gated hot runner tools process KKZ51C at melt temperatures of 210–230°C, mould coolant at 8–15°C, injection pressure 80–120 MPa, and hold pressure 50–70 MPa for 2–6 s depending on wall thickness. The addition ratio for still-liquid closures and industrial lids is 97.0–99.5 wt% KKZ51C, 0.5–2.5 wt% colour masterbatch, and 0.05–0.15 wt% antistatic additive where surface resistivity below 1×10^11 Ω is required for dry-flow handling. Compliance references are ISO 527-2:2012 tensile properties, ISO 179-1:2010 Charpy impact, ISO 1183-1:2019 density, FDA 21 CFR 177.1520 for food-contact olefin polymers, and EU 10/2011 overall migration requirements. Dimensional stability data from multicavity trials show flow-direction shrinkage of 1.5–2.5% and transverse shrinkage of 0.8–1.5%; tooling for tamper-evident bands must compensate for ovality generated by differential crystallisation after ejection. Hot runner nozzle temperatures are held within 210–230°C; cold-runner tooling is avoided for high-cavitation closure moulds because pressure loss across the runner generates inconsistent gate freeze-off. If pellet surface moisture is present from storage at relative humidity above 60%, pre-drying at 80°C for 2 h is required to avoid splay. Terminal finished products are screw closures for still liquids, tamper-evident caps, industrial pail lids, and thin-wall containers.
Water-bath tape lines with 75–120 mm single-screw extruders and T-dies from 900 mm to 1600 mm width convert KKZ51C into slit tape and monofilament at melt temperatures of 195–215°C, water quench temperature 25–40°C, and slit tape width 1.5–5.0 mm. Formula addition for outdoor woven sack and netting stock is 94.0–97.5 wt% KKZ51C, 2.0–4.0 wt% hindered amine light stabilizer masterbatch, and 0.5–1.0 wt% lubrication/processing aid to limit fibrillation before the draw section. Compliance is tested according to ISO 527-3:2018 tensile properties of film and sheet, ISO 2062:2009 tenacity of yarn, ASTM D2256 yarn elongation, and ISO 4892-3 QUV ageing cycles. The stretching sequence uses a first-stage draw ratio of 1:5.0 to 1:7.0 in a hot-air oven at 105–125°C, followed by a relaxation stage of 2–5% to reduce post-stretch shrinkage; excessive back tension at the winder can initiate splitting at the slit edge. Crease roller and slitting blade alignment must be maintained within 0.05 mm lateral runout; draw oven temperatures above 125°C cause surface oxidation and reduced tape tenacity. Terminal finished product types are woven packaging fabrics, agricultural netting, and industrial monofilament for rope and brush bristles.
Competitive TPC (Japan) HDPE KKZ51C prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
TPC (Japan) HDPE KKZ51C is a pelletised high-density polyethylene grade supplied for extrusion blow moulding of rigid containers, automotive reservoirs, industrial packaging and agrochemical bottles. The product is specified principally by melt mass-flow rate and density. Supplier-published typical data list a density of 0.956 g/cm³ when measured per ISO 1183-1 and a melt mass-flow rate at 190 °C and 2.16 kg of 0.35 g/10 min when measured per ISO 1133-1:2022. The high-load melt mass-flow rate at 190 °C and 21.6 kg is reported near 28 g/10 min. The resulting flow-rate ratio of approximately 80:1 indicates a broad molecular weight distribution typical of blow-moulding HDPE grades that must balance parison stability against extrusion backpressure.
The property set in Table 1 represents supplier-typical values for KKZ51C. These are not contractual specification limits; lot release is controlled by certificate of analysis for melt index, density, colour, contamination and moisture.
| Property | Test method | Typical value |
|---|---|---|
| Density | ISO 1183-1 | 0.956 g/cm³ |
| Melt mass-flow rate | ISO 1133-1:2022 | 0.35 g/10 min |
| High-load melt mass-flow rate | ISO 1133-1:2022 | 28 g/10 min |
| Tensile stress at yield | ISO 527-2 | 28.0 MPa |
| Tensile strain at break | ISO 527-2 | >600 % |
| Flexural modulus | ISO 178 | 1,300 MPa |
| Notched Charpy impact strength, 23 °C | ISO 179-1/1eA | 6.0 kJ/m² |
| Vicat softening temperature, A50 | ISO 306 | 125 °C |
| Shore D hardness | ISO 48-4 | 65 |
| Environmental stress cracking resistance, F50, 10% Igepal CO-630, 50 °C | ASTM D1693 | >100 h |
Part design exerts a first-order influence on KKZ51C performance. Minimum nominal wall thickness should be 0.8 mm for small bottles and 1.5 mm for industrial containers; local reductions below 0.7 mm at corners can lower drop-impact resistance and shorten environmental stress cracking failure time. Radius-to-wall-thickness ratios below 2:1 are avoided because they concentrate stress at moulded-in edges. A continuous bottle sidewall with gradual transitions from shoulder to body to base is preferred; threads and ribs should be located away from the parting line to maintain pinch-off strength.
Top-load strength is evaluated by vertical compression on empty or filled containers. For a 20 L container, a top-load target above 2,000 N is common; the actual value depends on wall thickness and shoulder radius. Stacking tests per ASTM D4169 or ISTA 3A are used for distribution trials. Published data for KKZ51C in specific top-load configurations is limited; customers generate performance data on the final article.
In machine selection, accumulator-head blow-moulding lines are preferred for parts exceeding 5 L because intermittent extrusion stores melt while the mould is closed. Melt temperature at the die is maintained between 190 °C and 210 °C. Cooling water temperature is set from 10 °C to 20 °C; mould surface temperatures above 25 °C reduce surface defects but lengthen cycle time. Blow air pressure is normally 0.6 MPa to 0.8 MPa after the pre-blow sequence. Pre-blow timing is adjusted so that the parison does not contact the mould cavity before full inflation, which would produce cold folds.
Barrier screws with compression ratios between 2.5:1 and 3.5:1 and length-to-diameter ratios from 24:1 to 30:1 are used. High-shear mixing sections are generally unnecessary; excessive shear can reduce melt strength through molecular orientation. On continuous-extrusion shuttle machines, melt pumps are used to stabilise pressure and parison length drift. Residence time above 240 °C should not exceed 20 min; longer residence can consume the stabiliser package and generate odour or gels.
Parison programming is required when part length exceeds 400 mm or minimum wall thickness falls below 1.0 mm. The die gap is varied during extrusion to increase wall thickness at the top pinch-off and bottom tail. For a 20 L jerry can with target minimum wall thickness of 1.2 mm, initial die gaps are commonly 1.8 mm to 2.4 mm on an 80 mm diverging die. A parison length of 650 mm may require 6 to 10 programming points. Melt temperature above 210 °C causes sag and a thin bottom; temperature below 180 °C increases melt elasticity, die swell, melt fracture and poor weld-line strength.
Die swell is measured as the ratio of parison diameter to die diameter at the die exit. For KKZ51C at 190 °C and shear rates typical of a 50 mm accumulator die, parison diameter is expected to be 1.3 to 1.5 times the die diameter; die swell above 1.8 indicates too low a melt temperature or excessive melt elasticity. Parison sag tests measure length change over time; a parison with length 600 mm should not exceed 15% length increase over 10 s. These values are machine-specific and must be established with the exact die geometry.
Mould closing speed influences pinch-off integrity. Closing speed is set between 0.2 m/s and 0.5 m/s for HDPE; slower closing may cause weak pinch-off and flash. Pinch-off insert geometry with tip radius below 0.5 mm creates stress concentration and is not used. A residual pinch thickness of 0.2 mm to 0.4 mm and smooth flash removal reduce crack-initiation sites at the parting line.
Batch melt mass-flow rate variation is controlled within ±0.05 g/10 min at 190 °C, 2.16 kg to maintain part-weight uniformity. A drift of +0.10 g/10 min in melt index can produce bottom flash and a weak sidewall under the same parison programme. Production shuttle machines with clamp forces from 15 t to 25 t typically hold part weight variation below ±1.5% when regrind ratio and hopper feed are stable.
Storage conditions influence lot consistency. HDPE is not hygroscopic, and pre-drying is usually unnecessary for unopened original packaging stored below 50 °C. If sacks are opened in a warehouse above 80% relative humidity, surface moisture can cause splay or melt surging; drying for 2 h at 80 °C with desiccant-air dew point below -20 °C is applied. Regrind is typically limited to 30 wt% in ESCR-sensitive applications. Above that level, loss of extensibility and ESCR is observed in ASTM D1693 F50 testing, and parison melt strength falls because recycled material has undergone additional thermal history.
Production-floor control includes hourly part-weight checks, wall-thickness mapping at the shoulder, sidewall and bottom, and low-temperature drop testing at -20 °C for automotive washer reservoirs. Leak testing of dangerous-goods packagings is conducted over 24 h at 40 °C with water when UN approval is required. Containers conditioned for 48 h at -20 °C are drop-tested from 1.2 m; embrittlement at the pinch-off is the main failure mode.
Substitution of KKZ51C into a PE100 pressure-pipe line is technically invalid. PE100 grades receive a long-term hydrostatic strength designation through ISO 12162 and are validated by ISO 9080. KKZ51C is not supplied with a PE100 designation; its molecular architecture supports parison stability and surface finish rather than slow crack growth resistance over decades. A pipe-grade HDPE with similar density may therefore have higher slow crack growth resistance even when short-term tensile values are comparable.
Compared with an injection-moulding HDPE with melt mass-flow rate above 10 g/10 min, KKZ51C exhibits high melt viscosity and is unsuitable for thin-wall closures or caps. The injection pressure needed to fill a 0.6 mm wall multi-cavity mould would exceed standard machine capacity because the low melt index limits flow length. If injection moulding is required, an HDPE grade with melt mass-flow rate above 4.0 g/10 min at 190 °C, 2.16 kg is normally selected. Compared with film-grade HDPE with density near 0.950 g/cm³ and melt index above 0.5 g/10 min, KKZ51C has higher density and lower melt index, giving greater top-load stiffness but a narrower blowing window. Published film-extrusion data for this specific configuration is limited because film lines are not the intended downstream route.
Comparative technical profiles are summarised in Table 2. Values are representative of the general grade classes and should not replace grade-specific data sheets.
| Parameter | KKZ51C blow-moulding grade | General-purpose injection HDPE | PE100 pipe HDPE | Blown-film HDPE |
|---|---|---|---|---|
| Density, ISO 1183-1 | 0.956 g/cm³ | 0.960 g/cm³ | 0.959 g/cm³ | 0.950 g/cm³ |
| Melt mass-flow rate, 190 °C, 2.16 kg | 0.35 g/10 min | 20 g/10 min | 0.25 g/10 min | 0.55 g/10 min |
| Flexural modulus, ISO 178 | 1,300 MPa | 1,600 MPa | 1,250 MPa | 1,000 MPa |
| ESCR F50, ASTM D1693 | >100 h | <10 h | >500 h | 50 h |
| Primary processing route | Extrusion blow moulding | Injection moulding | Pressure-pipe extrusion | Blown-film extrusion |
Chemical exposure and ESCR boundary conditions are critical in agrochemical and automotive packaging. ESCR is assessed with ASTM D1693 F50 in 10% Igepal CO-630 at 50 °C; the supplier-typical failure time exceeds 100 h. In containers for ester-based solvents, in-line fluorination is used to reduce permeation. Fluorine treatment is controlled to a surface fluorine uptake of 2 g/m² to 5 g/m² depending on container volume and solvent volatility. Without fluorination, hydrocarbon solvents with boiling points below 120 °C can permeate through HDPE at rates that may exceed regulatory packaging limits after 28 days at 40 °C.
Strong oxidising acids such as nitric acid above 30% concentration at temperatures above 40 °C cause oxidative degradation. Aromatic hydrocarbons, including toluene and xylene, swell HDPE; continuous immersion beyond 6 months is not recommended without barrier treatment. The effect of swelling on tensile modulus is measurable by ISO 527-2 after immersion in the target chemical at 40 °C for 90 days. Sharp corners below 0.8 mm wall thickness and pinch-off weld zones are the most common initiation sites for environmental stress cracking failures.
Food-contact declarations for KKZ51C are generally based on 21 CFR 177.1520 and EU Regulation 10/2011. End-use food-contact compliance is not automatically established by resin type; migration testing of the finished container is required because processing aids, regrind, colourants and fluorination treatments can change the final compliance profile. The grade is managed under REACH obligations and is not formulated with intentionally added phthalates.