| HS Code | 734327 |
| Polymer Type | PEN copolyester |
| Density | 1.33 g/cm³ |
| Glass Transition Temperature | 121 °C |
| Melting Temperature | 265 °C |
| Water Absorption | 0.30 % |
| Tensile Strength | 55 MPa |
| Elongation At Break | 2.0 % |
| Tensile Modulus | 2.4 GPa |
| Flexural Modulus | 2.3 GPa |
| Flexural Strength | 90 MPa |
| Notched Izod Impact | 0.030 kJ/m |
| Heat Deflection Temperature 0 46 Mpa | 100 °C |
| Heat Deflection Temperature 1 8 Mpa | 95 °C |
| Rockwell Hardness M | 95 |
| Mold Shrinkage | 0.50–0.70 % |
| Refractive Index | 1.65 |
| Visible Light Transmission | 88 % |
| Haze | 2 % |
| Dielectric Constant | 3.0 |
| Volume Resistivity | 1E16 Ω·cm |
As an accredited Toyobo Neostar® PEN Copolyester CNS-1 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg moisture-barrier bags, Toyobo Neostar® PEN Copolyester CNS-1 is supplied as pellets for industrial thermoplastic processing. |
| Container Loading (20′ FCL) | 20′ FCL container loading for Toyobo Neostar® PEN Copolyester CNS-1: palletized packages secured, evenly distributed, and stabilized for ocean shipment. |
| Shipping | Toyobo Neostar® PEN Copolyester CNS-1 is a non-hazardous copolyester resin/pellet. It is generally not regulated as dangerous goods under DOT, IATA, or IMDG. Ship in dry, closed containers at ambient temperature; protect from moisture, excessive heat, and direct sunlight. |
| Storage | Store Toyobo Neostar® PEN Copolyester CNS-1 in a cool, dry, well-ventilated area away from direct sunlight, heat, moisture, and ignition sources. Keep containers tightly closed and protect from dust, static, and UV exposure. Avoid prolonged storage above recommended temperatures and follow the manufacturer’s SDS and local regulations for safe handling and segregation. |
| Shelf Life | Shelf life is 24 months from manufacture when stored dry, cool, and in unopened original packaging away from direct sunlight. |
Competitive Toyobo Neostar® PEN Copolyester CNS-1 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Toyobo Neostar® PEN Copolyester CNS-1 is a naphthalate-based thermoplastic copolyester supplied as pellets for injection molding, sheet extrusion, extrusion blow molding, and injection stretch blow molding. The CNS-1 designation identifies a crystallisable grade in which the naphthalene-2,6-dicarboxylate backbone is interrupted by a proprietary comonomer. This modification lowers the crystalline melting point relative to homopolymer polyethylene naphthalate while retaining a glass transition temperature above conventional polyethylene terephthalate. Melt flow and thermal data are typically determined according to ISO 1133-1:2022, ISO 1183-1, and ISO 11357-1; tensile properties are commonly reported under ASTM D638-14. The grade is applied where transparent packaging must resist ester-based cosmetic ingredients, alcohol-based formulations, hot-fill conditions, or elevated ambient temperature without stress cracking. Grade-specific values for CNS-1 should be obtained from the current Toyobo technical datasheet because comonomer content, catalyst residues, and solid-state finishing affect crystallisation, melt viscosity, and barrier response.
Representative engineering data for naphthalate copolyesters of this class place glass transition temperature between 108 °C and 118 °C, crystalline melt point between 240 °C and 260 °C, and intrinsic viscosity between 0.65 dL/g and 0.80 dL/g. These ranges are class-typical values, not lot-specific certification. In comparison with PETG and PCTG, CNS-1-class copolyesters show lower oxygen permeability and lower environmental stress cracking in oils and alcohols; in comparison with homopolymer PEN, they reduce melt processing temperature and improve melt flow in thin-wall sections. The product is therefore positioned for applications that cannot use PETG because of chemical attack or barrier requirements and cannot use homopolymer PEN because of processing temperature constraints.
Food-contact status must be established for the specific grade and package construction. Naphthalate copolyesters may be evaluated under FDA 21 CFR 177.1630 for food-contact articles or under the consolidated EU 10/2011 framework for plastic materials intended to contact food. REACH Regulation (EC) No 1907/2006 and RoHS Directive 2011/65/EU declarations are supplier-specific and depend on catalyst residues and additives. Grade-specific documentation for CNS-1 should be requested from Toyobo before commercial use in medical, pharmaceutical, or food-contact devices.
Moisture uptake in naphthalate copolyesters is not a passive storage inconvenience; residual moisture above 0.005 wt% initiates hydrolytic chain scission during plasticating. Drying equipment for CNS-1 should maintain a dew point of -40 °C or lower and a hopper air temperature of 160 °C for 4 h to 6 h when pellets have been exposed to ambient conditions above 60% RH. Desiccant-bed dryers with closed-loop regeneration are preferred over hot-air units because the target equilibrium moisture for naphthalate copolyesters is below the capability of hot-air systems under humid plant conditions. On production-scale injection molding lines with 25 mm to 40 mm general-purpose screws, melt temperature should be maintained between 270 °C and 285 °C. Barrel profiles with a reverse temperature gradient in the feed zone reduce the risk of shear heating and localised naphthalene degradation. If melt residence time exceeds 8 min at 285 °C, yellowing and a measurable drop in intrinsic viscosity typically occur, indicating transesterification and chain scission.
Failure modes observed on injection lines include nozzle stringing, brown specks after 30 min interruptions, and variation in preform weight on hot-runner systems. Feedthroat cooling must be adjusted to prevent bridging because pellet softening begins near 100 °C and partial melting in the feed throat can restrict throughput. When a cold start is necessary, purging with a low-viscosity polyolefin or dedicated polyester purge compound at 280 °C is preferred; PVC purges are incompatible with naphthalate copolyesters and can generate acidic decomposition residues. If the feedthroat is too warm, pellets may agglomerate and cause a loss of screw feed, while excessive cooling can produce condensation that re-introduces moisture into the feed stream.
Injection stretch blow molding of CNS-1 preforms is carried out with preform surface temperatures in the 105 °C to 125 °C range. The crystallisable nature of the grade requires a narrow axial temperature profile because gradient amplitudes greater than 5 °C between the neck and gate produce sidewall thickness variation and local pearlescence from strain-induced crystallisation. Blow molds held at 120 °C to 140 °C permit controlled crystallisation in the finish and shoulder areas, improving chemical resistance and reducing post-mold shrinkage. Compared with PETG-type copolyesters, which remain amorphous in normal tooling, CNS-1 can be blown into containers with lower oxygen transmission and better shape retention after hot filling. Oxygen transmission is normally determined according to ASTM D3985, water vapour transmission according to ASTM F1249, and haze according to ASTM D1003. Class-typical oxygen permeability for this polymer family is roughly 3–5× lower than PET homopolymer at equal thickness. Processors should confirm orientation-induced barrier improvement on the actual preform design because local wall thickness and stretch ratios dominate the final barrier value.
For sheet extrusion of CNS-1, a 32:1 L/D single-screw extruder with a barrier screw and vacuum venting is typical. Melt temperatures of 270 °C to 285 °C and chill-roll temperatures of 80 °C to 110 °C produce amorphous or partially crystallised sheet depending on roll residence time. Thermoforming of CNS-1 sheet requires sheet surface temperatures near 120 °C to 140 °C; below this range the sheet springs back, and above this range crystallisation reduces detail reproduction. Tooling with aluminium or steel temperature control at 120 °C or higher is used when chemical resistance is required in the final article.
Homopolymer PEN exhibits a glass transition near 120 °C to 125 °C and a melt temperature above 265 °C, which forces extruder and injection barrel setpoints above 290 °C. CNS-1, by incorporating a proprietary comonomer in the naphthalate backbone, shifts the melting endotherm downward while retaining enough symmetry to crystallise under heated tooling. This separates it from PETG and PCTG, which use 1,4-cyclohexanedimethanol modification and remain amorphous under conventional processing. The practical consequence is that CNS-1 can be processed at temperatures closer to PET equipment capabilities than homopolymer PEN, yet it retains a higher glass transition temperature and lower oxygen permeability relative to PETG.
| Property | Test method | CNS-1 class-typical | Homopolymer PEN class-typical | PETG class-typical |
|---|---|---|---|---|
| Glass transition temperature | ISO 11357-2 | 108–118 °C | 120–125 °C | 78–82 °C |
| Melting endotherm | ISO 11357-3 | 240–260 °C | 265–270 °C | none |
| Density | ISO 1183-1 | 1.33–1.36 g/cm³ | 1.36 g/cm³ | 1.27 g/cm³ |
| Oxygen permeability | ASTM D3985 | 12–20 cm³·mm/m²·day·atm | 10–14 cm³·mm/m²·day·atm | 60–90 cm³·mm/m²·day·atm |
| Tensile strength | ASTM D638 | 70–80 MPa | 75–85 MPa | 50–55 MPa |
| Flexural modulus | ASTM D790 | 2400–2600 MPa | 2500–2800 MPa | 1900–2100 MPa |
The tabulated ranges represent class-typical engineering data and should not replace lot-specific certification. CNS-1’s combination of crystallinity and reduced melt point is particularly relevant for multi-cavity injection molding tools where hot-runner balance is critical. Compared with PETG, the grade shows higher melt strength and lower acid/alcohol permeability; compared with homopolymer PEN, it offers lower processing energy demand and reduced risk of thermal degradation in screw recovery. Melt flow rate should be interpreted under ISO 1133-1:2022 using a 2.16 kg load at 280 °C, because the value is highly sensitive to residual moisture and drying history. Differences in comonomer concentration can shift the glass transition by 3–5 °C and the melting point by 10–20 °C, which is why direct substitution between polyester grades without re-validation is not recommended.
Regrind use in CNS-1 containers is limited by the need to preserve intrinsic viscosity and low gel formation. Processing trials on 35 mm single-screw extruders with 24:1 L/D have shown that regrind addition above 30 wt% can generate thermal decomposition products and increase preform rejects when the regrind is not dried to below 0.005 wt% moisture. Regrind should be granulated from clean, non-contaminated scrap, stored in foil-lined bags, and reintroduced through a separate feeder to maintain a consistent melt viscosity. For coextrusion of barrier structures, CNS-1 can be used as a barrier layer with polyolefin skin layers, but adhesive resins must be selected for temperatures above 270 °C. The layer structure should be designed so that CNS-1 is not exposed to amine-containing tie resins that can catalyse transesterification and produce gel particles.
Die-lip build-up and plate-out are more prevalent when processing naphthalate copolyesters at high shear rates. Extruder screw speeds above 80 min⁻¹ on 30 mm general-purpose single-screw extruders may raise local melt temperature above 290 °C, resulting in gel particles and reduced layer clarity. Feedblock and die temperatures should be controlled independently to avoid thermal degradation in stagnant flow regions. Published data for this specific product grade in high-barrier coextrusion structures are limited; therefore, pilot-scale evaluation is required before specifying CNS-1 as a direct substitute for EVOH or polyamide barrier layers. Multilayer structures that combine CNS-1 with EVOH may show improved retort shock resistance, but interlayer adhesion and water absorption must be measured under ASTM F904 or equivalent.
Chemical resistance testing in cosmetic and personal-care packaging frequently uses immersion or fixed-strain tests with sunscreen agents, ethanol, isopropyl alcohol, and ester-based solvents. CNS-1-class naphthalate copolyesters show lower environmental stress cracking in alcohol-based formulations than PETG when evaluated under a fixed-strain jig method based on ISO 22088-3. Autoclave sterilisation at 121 °C for 20 min is possible for moulded parts with adequate wall uniformity, but repeated cycles may increase haze and reduce impact resistance because naphthalate copolyesters are sensitive to hydrolytic ageing. Gamma irradiation resistance of homopolymer PEN is typically higher than PET; however, published dose-response data for CNS-1 specifically are limited. In diagnostic and optical applications, the low autofluorescence of naphthalate copolyesters is often evaluated by excitation at 350–370 nm and emission beyond 400 nm; users should verify grade-specific fluorescence because comonomer residues can shift the background signal.
For converters currently running PETG on single-stage injection blow molding machines, conversion to CNS-1 requires raising barrel and hot-runner temperatures by roughly 20–30 °C, increasing mold temperature from 10–20 °C to 100 °C or higher to exploit crystallisation, and adding a high-temperature drying system. For converters evaluating homopolymer PEN, CNS-1 reduces barrel setpoints by 20–40 °C and improves flow in thin-wall sections. These operational differences are central to grade selection and should be validated on the specific machine configuration because clamp force, screw recovery time, and hot-runner balance vary with melt viscosity.