| HS Code | 829321 |
| Productname | Toyobo Neostar® PEN Bottle BN-1 |
| Model | BN-1 |
| Manufacturer | Toyobo Co., Ltd. |
| Material | Polyethylene naphthalate (PEN) |
| Capacity | 1 L |
| Bottletype | Narrow-mouth bottle |
| Color | Transparent |
| Closuretype | Screw cap |
| Autoclavable | Yes |
| Heatresistance | Autoclavable at 121°C |
| Chemicalresistance | High resistance to acids, alkalis, and organic solvents |
| Gasbarrier | High oxygen and carbon dioxide barrier |
| Uvprotection | Blocks ultraviolet light |
| Transparency | High transparency |
| Lowextractables | Low elution suitable for high-purity applications |
| Density | 1.36 g/cm³ |
| Waterabsorption | Low |
| Countryoforigin | Japan |
As an accredited Toyobo Neostar® PEN Bottles BN-1 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied as one bottle per pack, securely wrapped and boxed to protect Toyobo Neostar® PEN Bottles BN-1 during shipping. |
| Container Loading (20′ FCL) | A 20′ FCL shipment of Toyobo Neostar® PEN Bottles BN-1, securely palletized and loaded into a standard 20-foot container for ocean freight. |
| Shipping | Toyobo Neostar® PEN Bottles BN-1 are shipped as non-hazardous articles in sturdy, cushioned cartons. They are not regulated for transport (no UN number or hazard class). Handle carefully to prevent crushing or contamination; keep dry and store away from direct sunlight and heat. |
| Storage | Store Toyobo Neostar® PEN Bottles BN-1 in a cool, dry, well-ventilated area, away from direct sunlight, heat, sparks, flames, and incompatible chemicals. Keep containers tightly closed and upright in original packaging to prevent contamination or damage. Protect from physical impact, inspect periodically, ensure labels remain legible, and follow the manufacturer’s SDS and local regulations. |
| Shelf Life | Typical shelf life is 12 months from manufacture when kept sealed in original packaging at room temperature, away from sunlight. |
Competitive Toyobo Neostar® PEN Bottles BN-1 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Toyobo Neostar® PEN Bottles BN-1 is a polyethylene naphthalate copolymer resin supplied as cylindrical pellets for monolayer stretch blow molded containers and barrier-layer preforms. The grade is formulated for injection stretch blow molding, with a glass transition temperature near 120 °C, a crystalline melting peak between 260 °C and 270 °C depending on copolymer content, and a reported intrinsic viscosity in the bottle-grade range of 0.55 dL/g to 0.70 dL/g. Pre-drying in a desiccant dryer to a residual moisture level below 50 ppm using a supply air dew point of −40 °C or lower is mandatory; failure to maintain this moisture boundary will reduce melt viscosity through hydrolysis and can increase preform haze. The material is used when container specifications require gas barrier better than uncoated PET, resistance to distortion above 85 °C, retention of carbon dioxide in small-format beverage packages, or UV screening of light-sensitive liquid formulations. Published data for the BN-1-specific datasheet are limited; the following sections therefore use documented polyethylene naphthalate bottle-grade values and identify where grade-specific verification is required.
At molecular level, the replacement of a single terephthalate ring with a fused 2,6-naphthalenedicarboxylate unit stiffens the polymer backbone and reduces the segmental motions responsible for gas transport. This structural change raises the glass transition temperature by approximately 40 °C relative to bottle-grade PET and reduces oxygen permeability to roughly 20 % to 25 % of the PET value under ASTM D3985 at 23 °C and 0 % RH. Carbon dioxide permeability is reduced by a similar or slightly larger factor; published comparative data place PEN carbon dioxide transport at approximately 15 % to 20 % of PET under the same temperature and driving force. Water vapor transmission under ASTM F1249 at 38 °C and 90 % RH is approximately 25 % to 35 % of PET. The higher rigidity also increases tensile modulus; ISO 527-2 values for neat PEN bottle grades are typically 5.0 GPa to 5.5 GPa, compared with 2.8 GPa to 3.0 GPa for PET. These differences allow monolayer BN-1 containers to approach the gas barrier of multilayer structures while retaining a single-material construction.
Because the fused naphthalate ring absorbs ultraviolet radiation through 380 nm, BN-1 preforms and bottles screen UV more effectively than PET, which is largely transparent above 315 nm to 320 nm. The UV-blocking behavior is intrinsic to the polymer backbone and does not rely on surface coatings. However, the absorption of UV energy can increase resin yellowness during prolonged processing; therefore, hot-runner temperatures above 320 °C are avoided.
| Property | Bottle-grade PET | Neostar® PEN bottle grade | Test basis |
|---|---|---|---|
| Oxygen permeability normalized to PET | 1.0 | 0.20–0.25 | ASTM D3985, 23 °C, 0 % RH |
| Carbon dioxide permeability normalized to PET | 1.0 | 0.15–0.20 | Published comparative data, 23 °C, 0 % RH |
| Water vapor transmission normalized to PET | 1.0 | 0.25–0.35 | ASTM F1249, 38 °C, 90 % RH |
| Glass transition temperature | 76–80 °C | 120–125 °C | ISO 11357-2, 10 °C/min |
| Tensile modulus | 2.8–3.0 GPa | 5.0–5.5 GPa | ISO 527-2 |
Drying of BN-1 must be performed in desiccant dryers with supply air dew point no higher than −40 °C and pellet temperature between 150 °C and 170 °C for 5 to 6 hours. Residual moisture should be verified by Karl Fischer titration according to ASTM E203 or calibrated hygrometry and held below 50 ppm. A drying hopper with insulated transition to the feed throat is recommended to prevent moisture regain when ambient relative humidity exceeds 60 %. The melt processing window is higher than PET; barrel settings of 290 °C to 315 °C are typical, with nozzle temperature between 295 °C and 320 °C. A 24:1 or 25:1 screw with a low-shear barrier zone and reverse-flighted mixing section is used on preform injection machines. Hot-runner valve gate systems should be balanced to within ±2 °C across all cavities; greater thermal imbalance will produce preform melt flow variation that appears as weight dispersion and uneven sidewall thickness after blow molding.
Melt residence time above 310 °C should not exceed 5 minutes. Excessive residence time can generate aldehydes and volatile oligomers that read through as taste-odor defects or surface splay. Injection speeds should be set to fill the preform cavity in 0.5 s to 1.5 s for standard 28 mm neck finishes; fast injection may shear heat the naphthalate melt and create gate blush. Preform molds are cooled with chilled water at 2 °C to 8 °C, and cooling time is typically 12 s to 18 s for preforms with wall thickness from 3.0 mm to 4.5 mm. These values are equipment-specific and should be optimized on the preform line; published data for BN-1-specific cycle times are limited.
In reheat stretch blow molding, the preform surface must reach 130 °C to 150 °C because the higher Tg requires more thermal energy before stretching. Axial stretch ratios between 2.2:1 and 3.0:1 and hoop stretch ratios between 3.0:1 and 4.5:1 are applied; the resulting total areal stretch of 8:1 to 12:1 develops strain-induced crystallinity and sidewall orientation. Blow mold temperature is set from 80 °C to 120 °C for standard packages and from 120 °C to 160 °C for heat-set hot-fill containers. Venting slots of 0.03 mm to 0.05 mm depth in the blow mold are recommended to prevent trapped gas defects. Mold release pressure should be kept as low as practical to reduce stress whitening in the base and heel.
When BN-1 is co-injected with PET or another internal layer in a multilayer preform, the barrier layer must remain continuous around the bottle sidewall and base. The higher melt temperature of BN-1 relative to PET can create a viscosity mismatch in co-injection; melt temperature adjustments are required to prevent layer breakup or core-layer thinning. Published data for this specific configuration is limited, and process development should include cross-sectional microscopy of preforms and bottles to confirm layer continuity.
Melt viscosity of bottle-grade PEN is more temperature-sensitive than PET in the injection molding range. Processors should monitor intrinsic viscosity retention from pellet to preform by solution viscometry according to ISO 1628; a drop greater than 0.05 dL/g during drying and molding indicates hydrolysis or thermal chain scission and warrants a dew-point check of the drying system. The glass transition temperature of molded preforms should be confirmed by differential scanning calorimetry at 10 °C/min according to ISO 11357-2; amorphous preforms should show a clear Tg near 120 °C and minimal crystallization exotherm below 150 °C. Preform haze measured by ASTM D1003 should remain below 2 % for monolayer applications; higher haze indicates moisture-induced crystallinity or incompatible additives.
Comparative shelf-life calculations for monolayer carbonated beverage bottles show that replacing PET with BN-1 can extend the time to 15 % carbonation loss by a factor of 4 to 5 at equivalent wall thickness, or can allow a wall-thickness reduction of approximately 15 % to 20 % while retaining the same shelf life. For oxygen-sensitive beverages, lower oxygen ingress under ASTM D3985 conditions translates into slower vitamin C loss and reduced color change in accelerated storage at 30 °C and 50 % RH. These estimates assume the resin is processed without excessive amorphous orientation or moisture degradation; preforms with high residual moisture or IV loss will not reproduce the intrinsic barrier of the naphthalate backbone. Packaging engineers should validate barrier performance using finished bottle transmission rates, not resin permeability coefficients alone, because wall thickness distribution, induced crystallinity, and barrier-layer continuity control final package performance.
For filling temperatures between 85 °C and 95 °C, hot-fill processing places the package wall in a thermal range that is closer to the Tg of PET than to BN-1. Bottles made from BN-1 are dimensionally stable at these temperatures because the Tg near 120 °C provides a wider margin before thermal softening. Neck finish ovalization is minimized when the preform neck is crystallized to a density gradient typical of heat-set PET, but grade-specific process conditions must be developed. Heat-set blow molding holds the bottle against a heated mold at 120 °C to 160 °C for additional crystallinity; because PEN crystallizes more slowly than PET, longer mold contact times or higher mold temperatures may be required to stabilize the sidewall. If the mold is released too early, the bottle may exhibit excessive post-molding shrinkage and volume loss after filling.
Refillable containers are washed with 2 % to 3 % sodium hydroxide solution at 60 °C to 75 °C. The ester linkage in PEN is less susceptible to caustic-induced stress cracking than PET under these conditions, but concentrated alkali at temperatures above 80 °C can still reduce intrinsic viscosity and should be avoided. Base and shoulder radii should be designed with generous radii, and top-load testing according to ASTM D2659 should be performed before and after simulated caustic wash cycles to assess crack propagation. Impact resistance after hot-fill should be evaluated by filled drop impact using ASTM D2463; the higher stiffness of PEN may reduce ductile deformation in thin sections, so minimum wall thickness should not be set below the point where environmental stress cracking resistance is maintained. Published data for BN-1-specific repeated caustic wash performance is limited; validation on the intended filling line is required.
Moist-heat retort sterilization at 121 °C for 30 minutes generally exceeds the practical continuous dimensional stability limit of monolayer PEN bottles; such applications require multilayer structures with polypropylene or metal barriers, and BN-1 would not be selected as the sole structural layer.
Relative to multilayer EVOH preforms, BN-1 avoids the use of adhesive tie layers and retains oxygen barrier at high humidity; EVOH oxygen transmission can rise by an order of magnitude when equilibrated at 90 % RH, while PEN is hydrophobic and does not undergo the same moisture-induced barrier loss. Against MXD6 nylon blends, PEN provides higher optical clarity and lower haze, since nylon domains above 5 % to 10 % addition can scatter light and increase yellowness. Compared with silicon oxide or carbon-coated PET, BN-1 eliminates the secondary vacuum coating line and the risk of flex-induced coating cracks, but the resin cost is higher and the preform reheat window is narrower. Glass and aluminum provide lower absolute gas and moisture transmission but require different sealing, retort, and recycling infrastructure. Selection is therefore based on whether the required shelf life, hot-fill temperature, and filling-line compatibility justify the higher resin cost of a monolayer naphthalate container.
Before food-contact commercialization, converters must confirm that BN-1 complies with the relevant regulations. In the European Union, plastic food-contact articles are tested under Regulation (EU) No 10/2011; overall migration must not exceed 10 mg/dm² under the prescribed simulants and time-temperature conditions. Specific migration limits for 2,6-naphthalenedicarboxylic acid and any co-monomers or additives must be checked against the latest consolidated list. In the United States, food-contact status for polyethylene naphthalate may be covered by Food Contact Notifications or other premarket clearances; the absence of a dedicated 21 CFR citation for BN-1 means that supplier documentation must be retained. Japan, China, and Mercosur have additional positive-list requirements, and pharmaceutical use may require USP General Chapter 661.1 or 661.2 testing for plastic containers.
| Requirement | Test or standard designation | Typical control boundary | Verification point |
|---|---|---|---|
| Overall migration, EU plastic FCM | Regulation (EU) No 10/2011, Annex III | ≤10 mg/dm² | Finished bottle or preform |
| Oxygen transmission | ASTM D3985 | Final bottle OTR; design-dependent | Conditioned bottle, 23 °C, 0 % RH |
| Water vapor transmission | ASTM F1249 | Final bottle WVTR; design-dependent | 38 °C, 90 % RH |
| Tensile modulus | ISO 527-2 | 5.0–5.5 GPa | Dumb-bell specimen from molded sheet |
| Glass transition | ISO 11357-2 | 120–125 °C | DSC, 10 °C/min |
| Intrinsic viscosity | ISO 1628 | Supplier specification; typically 0.55–0.70 dL/g | Pellet and preform |
| Caustic stress cracking | ASTM D2659 top-load after caustic wash | No visible cracks; top-load retention target design-specific | Finished bottle, simulated wash |
Extraction studies should be performed on finished preforms or bottles, not only on pellets, because processing can generate oligomers at the surface. Standard extraction protocols include aqueous, 3 % acetic acid, 10 % ethanol, and fatty-food simulants under time-temperature conditions defined in Regulation (EU) No 10/2011. For pharmaceutical syrups and topicals, drug product stability protocols per ICH Q1A are used to detect active ingredient sorption into the container wall or leachables migrating into the liquid. Heavy-metal and SVHC compliance under RoHS and REACH is confirmed through supplier declarations, but sulfur-containing processing aids or colorants can introduce restricted substances and must be controlled at the conversion site.