| HS Code | 477478 |
| Material Type | High Density Polyethylene (HDPE) |
| Color | Black |
| Density | 0.946 g/cm³ |
| Melt Flow Rate | 0.20 g/10 min (190°C/2.16 kg) |
| Melting Point | 131 °C |
| Vicat Softening Temperature | 122 °C |
| Tensile Strength At Yield | 24 MPa |
| Tensile Strength At Break | 32 MPa |
| Elongation At Break | >600% |
| Flexural Modulus | 1100 MPa |
| Notched Charpy Impact Strength | 15 kJ/m² |
| Shore D Hardness | 60 |
| Environmental Stress Cracking Resistance | >1000 h |
| Carbon Black Content | 2.0% |
| Brittleness Temperature | < -70 °C |
As an accredited TotalEnergies HDPE 4206B BK factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | TotalEnergies HDPE 4206B BK is supplied in 25 kg polyethylene bags, typically 55 bags per pallet (1,375 kg). |
| Container Loading (20′ FCL) | 20′ FCL loaded with TotalEnergies HDPE 4206B BK in 25 kg bags, palletized, shrink-wrapped, strapped, securely stowed for ocean transport. |
| Shipping | TotalEnergies HDPE 4206B BK is shipped as non-hazardous, solid black polyethylene pellets in moisture-barrier bags, octabins, or bulk containers. It requires no dangerous goods documentation. Keep dry, away from heat, sunlight, and contamination. Standard industrial handling and transport apply. |
| Storage | Store TotalEnergies HDPE 4206B BK in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, ignition sources, and incompatible chemicals. Keep original packaging closed and palletized, off the ground, to prevent moisture, dust, oil, solvent, acid, or alkali contamination. Avoid prolonged UV exposure and excessive stacking. Follow first-in, first-out stock rotation. Do not store outdoors. |
| Shelf Life | TotalEnergies HDPE 4206B BK has no defined shelf life; store cool, dry, sealed, away from sunlight, heat, and contaminants. |
TotalEnergies HDPE 4206B BK is transferred directly to the extruder hopper of a 60–90 mm single-screw blow moulding machine with a grooved feed bushing and a 24:1–28:1 L/D screw. The barrel profile from feed throat to metering zone is held at 170–190 °C, while the accumulator head and die are trimmed to 195–205 °C. Screw speed is restricted to 40–70 rpm and back pressure is kept below 10 MPa to prevent carbon black agglomeration. The resin’s high-load melt flow rate under 21.6 kg load at 190 °C is the primary control variable for parison hang length. Where parison length exceeds 800 mm, die gap is reduced to 0.8–1.1 times the target wall thickness to compensate for draw-down. Blow pressure of 0.65–0.75 MPa is applied after a pre-clamp delay of 8–10 s. Cooling water at 10–12 °C is circulated through the mould core and cavity; demoulding is initiated when the part wall temperature falls below 85 °C. This process sequence is used for 20–30 L UN-certified jerrycans and industrial detergent containers. The black compound already contains carbon black at a dispersion level sufficient for outdoor UV resistance without a secondary masterbatch. Carbon black dispersion is checked under ISO 18553:2002, with a retained rating of ≤ 2.5 for lot acceptance. Drop testing after conditioning at −18 °C is conducted on filled and sealed containers according to ASTM D2463-15 and ADR 6.1.5.3. The same containers are evaluated for environmental stress-crack resistance under ASTM D1693-15 Condition B, with failure recorded only when two parallel cracks propagate through the wall within the tabulated test period.
Corrugated duct made from TotalEnergies HDPE 4206B BK runs without a separate carbon black masterbatch, so the melt pressure at the extruder die should not exceed 25 MPa to prevent additive agglomeration at the breaker plate. A 50–75 mm single-screw extruder with a 30:1 L/D screw feeds a corrugator at a melt temperature of 200–215 °C. The vacuum forming blocks are held at −0.2 to −0.4 bar relative to atmospheric pressure, and the mould block temperature is kept between 45 °C and 60 °C through closed-loop oil heating. Wall thickness for IEC 61386-24 compliant conduits is typically 1.2–3.2 mm, depending on nominal outside diameter. In-line regrind of the perforated corrugator start-up scrap is limited to 10 wt%, because higher closed-loop regrind fractions reduce the high-load melt index stability and produce visible surface streaks. Throughput is controlled by a gravimetric feeder to maintain ± 0.5 % mass per meter of finished duct. The finished duct is tested for compression strength and impact at −5 °C under IEC 61386-24:2020. The black compound satisfies RoHS limits for lead, mercury, cadmium, and hexavalent chromium under EU 2011/65/EU Annex II. REACH SVHC screening is generally limited to carbon black-derived PAHs under EC 1907/2006 Annex XVII. Published data for this specific corrugated duct configuration with 4206B BK are limited outside the converter’s internal extrusion records.
Extruded sheet from TotalEnergies HDPE 4206B BK is produced on a 90–120 mm single-screw sheet line with a barrier screw and a horizontal three-roll stack. Die temperatures are kept at 205–220 °C, and the roll gap is set to 1.5–4.0 mm for automotive wheel arch liner stock. The chill rolls are maintained at 35–55 °C to control crystallinity and to avoid warpage during downstream plug-assisted forming. Extruder back pressure is limited to 15 MPa to reduce shear heating of the black compound. Sheet surface temperature before forming is brought to 150–165 °C using twin infrared heating banks; the thermoforming mould is heated to 60–80 °C. Plug speed is limited to 200–400 mm/s to avoid local thinning at the wheel arch draw core. The formed parts are trimmed on a CNC five-axis router, and in-process regrind is reintroduced at up to 30 wt% with virgin material. This regrind fraction is monitored by melt flow rate testing under 21.6 kg load and 190 °C after each shift. The formed wheel arch liners are tested for low-temperature notch impact after conditioning at −30 °C for 24 h; acceptance criteria reference ISO 179-1:2010 Charpy notched impact and ISO 8256-1:2004 tensile impact. Tensile properties are measured according to ISO 527-2:2012. For passenger-cabin-adjacent parts, flammability is assessed under ISO 3795:1989 with a burn rate threshold defined by the vehicle manufacturer.
The comparative processing matrix below consolidates the melt temperature windows, critical control thresholds, and test methods used for the downstream routes described above.
| Downstream route | Nominal melt temperature | Critical control parameter | Primary standard |
|---|---|---|---|
| Extrusion blow moulding, 20–30 L containers | 195–205 °C at die | Parison hang length 600–900 mm | ASTM D2463-15; ADR 6.1.5.3 |
| Corrugated cable duct | 200–215 °C | Vacuum −0.2 to −0.4 bar | IEC 61386-24:2020 |
| Extruded sheet for thermoforming | 205–220 °C | Plug speed 200–400 mm/s | ISO 179-1:2010; ISO 8256-1:2004 |
| Spiral-wound drainage pipe | 195–210 °C | Melt string contact 0.15–0.30 MPa | ISO 9969:2016; ISO 9967:2016 |
| Thermoformed boot liners | 200–215 °C | Regrind 25–30 wt% | ASTM D1693-15; VDA 277:1995 |
For large-diameter spiral-wound pipe, TotalEnergies HDPE 4206B BK is extruded through a 50–70 mm profile die into a rotating drum winder. The melt strand is deposited at 195–210 °C onto the previously welded convolution. The drum surface is preheated to 40–60 °C with infrared panels to prevent cold-joint formation. The weld line temperature is verified with an infrared pyrometer at 200 °C before the compression roll. The winding pitch is adjusted to produce pipe with an internal diameter of 300–1,200 mm, and the strand compression roller applies 0.15–0.30 MPa contact pressure. The finished pipe is butt-fusion welded at 220 ± 5 °C using a hydraulically controlled welding machine; the fusion pressure is held at 0.15 MPa during the heating phase and released during the soak phase. Ring stiffness is measured under ISO 9969:2016 and creep ratio under ISO 9967:2016. The black compound provides UV stabilization for outdoor storage of pipe sections. However, published data for this specific spiral-wound configuration with 4206B BK are limited outside the manufacturer’s standard pipe test reports. The material should not be processed above 230 °C, because higher melt temperatures risk visible degradation of carbon black dispersion and a measurable drop in hot-tack string strength.
Black HDPE 4206B BK is used in automotive boot liners and luggage-compartment trays because the material tolerates closed-loop thermoforming regrind without losing dimensional stability. Extruded sheet is run at a melt temperature of 200–215 °C and is fed into a contact-heat thermoforming press. The sheet is preheated to 158–168 °C, and the forming plug is coated with a PTFE release layer to reduce sticking of the black compound. Oven residence time is 180–240 s for 2.5 mm gauge sheet. The tooling is water-cooled to 45–65 °C to stabilize the final grain depth. Regrind generated from trim stations is passed through a screen changer with a mesh size of 120 µm and reintroduced at 25–30 wt%. The melt flow rate of the blend is measured every 2 h under 21.6 kg load and 190 °C; a deviation greater than ± 10 % from the virgin lot value triggers replacement of the regrind feeder. Finished parts are subjected to a 48 h environmental stress crack resistance test in 10 % Igepal CO-630 solution at 50 °C, following the test geometry of ASTM D1693-15. The same parts must pass a flat-unfold extraction test for volatile organic compounds if they are installed in the passenger cabin; the test method is VDA 277:1995 total emission. In multi-layer constructions involving an outer polypropylene film, the polyethylene substrate contributes to formability but published adhesion values for this exact construction remain limited.
Competitive TotalEnergies HDPE 4206B BK prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
TotalEnergies HDPE 4206B BK is a black-pigmented, high-molecular-weight high-density polyethylene supplied as pellets for extrusion blow molding of rigid containers, jerry cans, automotive technical parts, and opaque packaging. The base grade is designed for high melt strength and long-term environmental stress crack resistance; the black color package is obtained with carbon black. Product-specific release values are controlled by the manufacturer’s current certificate of analysis. The standard characterization suite includes density by ISO 1183-1, melt mass-flow rate by ISO 1133-1, tensile properties by ISO 527-2, environmental stress crack resistance by ASTM D1693 or ISO 22088-3, carbon black content by ISO 6964, and carbon black dispersion by ISO 18553. In black high-molecular-weight HDPE blow-molding grades of this general class, density normally lies between 0.949 g/cm³ and 0.955 g/cm³, and melt mass-flow rate at 190 °C/2.16 kg normally lies between 0.30 g/10 min and 0.60 g/10 min. The exact HDPE 4206B BK release limits should be confirmed against the lot-specific datasheet.
The grade’s processing performance is governed by its melt rheology. At low shear rates relevant to parison hang time, high-molecular-weight chains increase elongational viscosity and resist sag; at higher die shear rates, shear thinning permits flow through the annular die. This combination supports stable parison formation without requiring excessive melt temperature. Environmental stress crack resistance is linked to the presence of long chains that form tie molecules between lamellae and resist fibril rupture at the base of a notch. A lower melt mass-flow rate generally indicates higher ESCR and improved drop impact resistance, but also higher die pressure and slower extrusion. Zero-shear viscosity at 190 °C may range from 10⁴ Pa·s to 10⁵ Pa·s, while viscosity at die shear rates of 10²–10³ s⁻¹ may fall to 200–400 Pa·s. The resulting shear-thinning ratio is exploited in blow molding: the parison retains shape after exit from the die, while flow through the die remains practical. Die swell may reach 1.5–2.5 depending on die geometry and output. These values are not release specifications but represent the rheological envelope for high-ESCR blow-molding HDPE.
| Property/control parameter | Test method | Typical class acceptance band | Notes for HDPE 4206B BK |
|---|---|---|---|
| Density at 23 °C | ISO 1183-1 | 0.949–0.955 g/cm³ | Higher density increases stiffness; excessive density may reduce ESCR |
| Melt mass-flow rate | ISO 1133-1 | 0.30–0.60 g/10 min | Measured at 190 °C/2.16 kg; lower values favor ESCR |
| Tensile yield stress | ISO 527-2 | 23–27 MPa | Relevant for rigid container top-load and handling |
| Elongation at break | ISO 527-2 | > 600% | Indicates ductile behavior under tensile deformation |
| Environmental stress crack resistance | ASTM D1693, ISO 22088-3 | > 1000 h F50 typical for high-ESCR grades | Accelerated test in 100% Igepal at 50 °C |
| Carbon black content | ISO 6964 | 2.0–2.5 wt% | Provides UV stabilization and opacity |
| Carbon black dispersion | ISO 18553 | rating ≤ 3 | Poor dispersion can create impact-initiated crack sites |
The table values are class-typical acceptance bands for black high-molecular-weight HDPE blow-molding feedstocks. They are not a substitute for the certified release values of TotalEnergies HDPE 4206B BK. For qualification work, the manufacturer’s current datasheet should be used for lot release, while part-level testing should be carried out on actual molded containers.
On a shuttle blow molding machine producing a 20 L jerry can, melt temperature is usually set between 190 °C and 210 °C at the die head. At melt temperatures above 220 °C, parison sag increases wall-thickness variation beyond ±0.3 mm; below 180 °C, surface defects such as shark skin and die lines can appear at high output. A barrier screw with L/D 24:1–30:1 and an accumulator head is used for larger containers, while continuous shuttle equipment is suitable for smaller parts. Mold cooling water is held at 8–15 °C; blow air pressure is typically 0.6–0.8 MPa. HDPE is non-hygroscopic, with moisture uptake generally below 0.01 wt% at 23 °C/50% RH, but surface condensation from outdoor storage can produce microvoids. If surface moisture is present, hopper drying at 70–75 °C for 2–4 h is sufficient; temperatures above 80 °C can soften pellets and cause feed bridging. A screen pack of 20/40/60 mesh and a melt pump pressure below 180 bar are typical safeguards. Batch-to-batch MFR variance within ±0.05 g/10 min is considered normal and may require only minor die temperature adjustment; larger variations can alter pinch-off weld strength and container top-load consistency.
Carbon black at 2.0–2.5 wt% functions as a UV absorber and radical trap, reducing embrittlement from outdoor exposure. Dispersion is controlled to a rating of ≤ 3 per ISO 18553 to limit agglomerates above 0.5 mm that act as stress concentrations. UV ageing comparisons are commonly performed under ISO 16871 or ASTM D2565, with retention of elongation at break used as the primary acceptance criterion. The BK variant provides opacity and light-barrier performance, but black surfaces also absorb infrared more readily during heating processes. Hot-plate welding, infrared welding, or preheating steps may therefore require slightly shorter soak times or lower heater outputs than unpigmented HDPE. If food-contact or potable-water certification is relevant, carbon black composition and migration limits must be confirmed under EU 10/2011 and FDA 21 CFR 177.1520. Solvent-based cleaning agents and aggressive chemical formulations can reduce ESCR unless compatibility is verified by immersion testing according to ISO 175 or ASTM D543.
Substitution in existing tooling requires revalidation of wall thickness distribution, pinch-off geometry, and cycle time. Because high-molecular-weight HDPE has lower flow, the extruder may run at higher pressure or require 5–10% lower screw speed to avoid melt fracture. The die gap and core pin may need adjustment to maintain parison diameter and wall uniformity. In accelerated ESCR testing under ASTM D1693 or ISO 22088-3, a high-ESCR grade may show failure times above 1000 h, whereas a standard HDPE blow-molding grade with MFR 1.0–1.5 g/10 min may fail between 50 h and 300 h. The improved ESCR allows downgauging in non-load-bearing packaging only when drop impact and top-load requirements remain satisfied. Compared with a natural HDPE blow-molding grade from the same family, the BK variant adds UV weathering resistance but reduces light transmittance and can alter recyclate color. It is not a pressure-pipe grade and should not be substituted into piping systems designed under ISO 4427 or ISO 4437. For industrial chemical containers, compatibility with the intended fill must be tested under ISO 175 or ASTM D543 because laboratory ESCR data cannot replace chemical compatibility trials.
| End-use condition | Standard/regulatory reference | Verification focus |
|---|---|---|
| Food-contact packaging | EU 10/2011; FDA 21 CFR 177.1520 | Overall migration and carbon black/additive migration limits |
| UV weathering | ISO 16871; ASTM D2565 | Retention of elongation at break after xenon/UV exposure |
| Environmental stress crack resistance | ASTM D1693; ISO 22088-3 | F50 failure time at 50 °C in 100% Igepal |
| Chemical compatibility | ISO 175; ASTM D543 | Tensile and mass change after immersion in service fluid |
| Heavy metals restrictions | RoHS 2011/65/EU | Pb, Hg, Cr VI, PBB, PBDE 0.1 wt%; Cd 0.01 wt% |
| Industrial container certification | UN Model Regulations; ADR/RID/IMDG | Drop, leak, stack, and hydraulic pressure testing of molded container |
Published data for this specific black coloration in continuous contact with aggressive agrochemical formulations is limited. Container qualification should include pre-production chemical compatibility trials and stress-cracking evaluation on molded parts. Avoid strong oxidizing acids, halogens, and aromatic solvents unless long-term compatibility is demonstrated. Do not blend with polyamide or EVOH barrier layers without a tie-resin, because delamination or weld-line weakness may develop. If outdoor storage is required, the black pigment package provides UV resistance only when carbon black content and dispersion remain within the specified bands. Product-specific values remain defined by TotalEnergies’ current certificate of analysis.