    Specifications
    HS Code 359015
    Polymertype High-density polyethylene (HDPE)
    Density 0.950 g/cm³
    Meltmassflowrate 0.05 g/10 min (190°C/2.16 kg)
    Tensilestressatyield 24 MPa
    Tensilestrainatbreak 500%
    Flexuralmodulus 1100 MPa
    Notchedizodimpactstrength 150 J/m at 23°C
    Vicatsofteningtemperature 122°C
    Meltingtemperature 131°C
    Shoredhardness 62
    Environmentalstresscrackingresistance >1000 h
    Waterabsorption <0.01%
    Thermalexpansioncoefficient 1.2E-4 1/°C

    As an accredited Tosoh HDPE HMS100 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Tosoh HDPE HMS100 is packaged in 25 kg paper bags, palletized and shrink-wrapped, with optional 1,000 kg jumbo bags.
    Container Loading (20′ FCL) Tosoh HDPE HMS100 loaded in clean, dry 20′ FCL: palletized bags, shrink-wrapped, evenly distributed, secured for safe ocean transport.
    Shipping Tosoh HDPE HMS100 is a non-hazardous high-density polyethylene resin shipped as solid pellets in 25 kg bags, bulk bags, or bulk trucks/railcars. Keep packaging closed and dry, protecting contents from heat, sunlight, moisture, and contamination. It is not DOT/UN regulated for transport under normal conditions. No special handling beyond standard chemical hygiene.
    Storage Store Tosoh HDPE HMS100 in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep containers tightly closed and palletized to prevent moisture, dust, and contamination. Avoid contact with strong oxidizers. Store away from acids, bases, and incompatible materials. Use original packaging and follow SDS. Ensure containers are labeled.
    Shelf Life Store in a cool, dry, ventilated area away from sunlight; typical shelf life is 24 months in unopened original packaging.
    Application of Tosoh HDPE HMS100

    Extrusion blow moulding of automotive fuel tanks from Tosoh HDPE HMS100 is executed on an accumulator-head machine with a 120 mm grooved-feed single-screw extruder at a 24:1 to 30:1 L/D ratio, because the resin’s high molecular weight provides parison stability during hang times exceeding 60 s. The melt temperature at the die bushing is held between 200°C and 220°C; the die gap is opened from 2.0 mm to 6.0 mm during parison extrusion to compensate for swell. HMS100 is dosed as the continuous matrix at 100 phr of the olefinic polymer phase for the outer and inner layers of six-layer barrier tanks; carbon black masterbatch is added at 0.5–2.0 phr and a hindered phenolic/phosphite stabilizer package at 0.05–0.15 phr. In tanks requiring hydrocarbon permeation resistance, a middle ethylene-vinyl alcohol copolymer barrier layer is coextruded at 2.0–4.0% of total wall thickness, with maleic anhydride-grafted polyethylene tie layers at 0.5–1.5% on either side. Compliance is demonstrated under UN ECE R34, including the fire resistance test of Annex 5, supplemented by ASTM D638-22 tensile yield and ASTM D256-23 notched Izod impact tests on cut plaques. Production-scale bottlenecks include chime-wall thinning below 2.5 mm at the joint transition and pin-flash tearing when the mould temperature falls below 12°C; the preferred mould shell temperature is 12–18°C with cooling water at 6–10°C. Blow air pressure is set to 0.6–1.0 MPa, clamp force between 150 and 400 tons, and total cycle time for a 60 L tank ranges from 120 to 200 s. The unit fails as a monolayer barrier under LEV III/China 6 evaporative emission limits if coextrusion is omitted. Terminal parts include 55–100 L gasoline and diesel fuel tanks, SCR urea reservoirs, and integrated fuel-filler spout bodies.

    What Accumulator-Head Parameters Preserve Drop-Impact Integrity in UN-Certified 220 L Tight-Head Drums?

    For UN 1H1/Y1.9/250 tight-head drums, the HMS100 fraction is introduced as the virgin resin stream at 100 phr, with carbon black masterbatch at 2.0–2.5 phr for ultraviolet stabilization and zinc stearate internal release at 0.05–0.10 phr; regrind from flash and rejected drums is reintroduced at up to 30 phr only after passing melt filtration through a 120/80/60 mesh pack. The process uses a 90 mm single-screw extruder with a 30:1 L/D barrier screw and an accumulator-head blow moulder; melt temperature is maintained at 190–210°C, while the parison programmer deploys 15–30 position points to increase wall thickness at the top chime and bottom chime to 4.0–5.0 mm and keep mid-sidewall at 1.8–2.2 mm. Blow pressure is 0.7–1.0 MPa, mould temperature is 8–15°C, and post-extrusion cooling is extended until the pinch weld reaches 60°C before demoulding. Type approval requires drop testing from 1.2 m at -18°C onto the side seam, chime, and closure in accordance with Chapter 6.1.5 of the UN Model Regulations, plus stacking tests at 50°C to verify no deformation beyond specified limits. ASTM D2463-23 establishes puncture resistance under static load, while ASTM D256-23 notched Izod provides quality assurance on specimens cut from the sidewall. A recurrent production failure mode is seal-area thinning at the flash line when the accumulator head is operated beyond a 70% shot capacity; limiting shot utilisation to 55–70% of the head volume preserves wall uniformity. Terminal products include 120 L, 200 L, and 220 L open-head and tight-head drums for liquid chemicals, viscous resins, and hazardous preparations requiring UN packaging certification.

    Flat-die sheet extrusion of HDPE geomembrane with HMS100 as the primary binder is carried out on a 150 mm single-screw extruder with a 30:1 L/D barrier screw and a continuous belt screen changer; melt temperature entering the die is held at 215–235°C to limit gel-phase defects from the high molecular weight tail. The formulation adds carbon black masterbatch at 2.0–3.0% total carbon black by mass, a hindered phenolic/phosphite antioxidant package at 0.05–0.2 phr, and a polymer processing aid at 0.01–0.05 phr; recycled resin is excluded when GRI GM13 conformance is specified. The melt exits a flat die with restricted tees and a choker bar into a three-roll calendering stack heated to 60–90°C; thickness is controlled from 0.75 mm to 3.0 mm by beta-gauge feedback and bolt-adjustable die lips. Draw ratio is held at 1.05–1.15 between die exit and cooling roll to minimise frozen-in orientation that would otherwise lower stress-crack resistance. Quality assurance uses ASTM D1505-18 for density, ASTM D1238-23 for melt flow ratio stability, ASTM D6693-22 for wide-width tensile, ASTM D5397-20 for single-point notched constant tensile load, and ASTM D4218-20 for carbon black content. A known processing boundary is the tendency for the high molecular weight resin to form sharkskin at melt temperatures below 210°C; increasing the die-lip temperature to 225°C and maintaining a 1.15:1 draw ratio suppresses the defect. Terminal products are single-ply HDPE geomembranes in 1.0 mm, 1.5 mm, 2.0 mm, and 3.0 mm thicknesses for municipal solid waste landfill basal and capping liners, mining heap-leach pads, evaporation ponds, and coal-ash impoundment liners.

    Thermoformed Heavy-Gauge HDPE Dunnage: Vacuum Draw Ratio and Hot-Sheet Sag Limits

    Heavy-gauge thermoforming of HMS100 begins with sheet extrusion at 8–15 mm thickness on a 120 mm single-screw extruder with a 30:1 L/D screw and a vertically adjustable flexible-lip sheet die; melt temperature is 200–220°C and roll-stack temperature is 70–90°C to eliminate internal vacuum voids. The formulation is 100 phr HMS100 with regrind at 10–30 phr, an external lubricant package at 0.05–0.1 phr, and 0.5–1.0 phr colour masterbatch if opaque black or grey sheet is specified. Sheet surface temperature at the thermoformer is monitored by infrared pyrometer and must fall within 165–190°C before vacuum is applied; top and bottom quartz ovens are set to 210°C and 190°C respectively, and sheet sag is limited to 5–10% of the clamp-frame span to prevent excessive wall thinning. The mould is aluminium, temperature-controlled at 35–55°C, and the vacuum system is pulled to 0.05–0.08 MPa within 1.5 s; draw ratios are constrained to 1.2:1–2.0:1 for reusable load-bearing parts. Test data are generated under ASTM D638-22 for tensile yield, ISO 6603-2:2018 for multi-axial impact puncture, and ASTM D2582-21 for puncture-propagation tear. When deep pockets exceed 150 mm, plug-assisted pre-stretch is required to bring the minimum corner thickness above 2.0 mm; otherwise corner puncture under cyclic returnable-packaging handling occurs. Terminal product forms include automated automotive body-in-white dunnage trays, returnable separator pallets for camshaft and battery modules, and heavy-gauge tote liners used in sequenced parts delivery.

    In agricultural chemical storage, large horizontal tanks are converted from HMS100 on accumulator-head blow moulders with a 150 mm grooved-feed extruder at a 30:1 L/D ratio and a first-in, first-out accumulator head sized for 10–30 kg shots. HMS100 is charged at 100 phr as the structural resin, with carbon black masterbatch at 2.0–2.5 phr for outdoor service and a hindered amine light stabilizer at 0.10–0.25 phr; filler, plasticizer, and recycled post-consumer resin are excluded from the wall compound for ASTM D1998-21 conformance. The melt temperature at the die is 190–210°C, parison programming uses 20–40 points to maintain a 3.0–4.0 mm bottom wall and 2.5–3.0 mm sidewall, mould temperature is 8–15°C, and clamp force for a 1,200 L horizontal tank is 400–800 tons. Internal blow pressure is 0.6–1.0 MPa, with an internal air-cooling sequence that begins at 60°C wall temperature and reduces tank bowing after demoulding; total cycle time ranges from 300 to 600 s depending on shot mass. The production-scale limitation is the risk of pinch-off tail weld cracking when the flash is trimmed below 15°C; trimming at 20–25°C after a 10-minute cooling rest reduces this. Terminal products are 600–1,500 L agricultural sprayer tanks, fertiliser injection tanks, seed-treatment mix tanks, and fresh water transport tanks mounted on trailed or skid platforms.

    When Cut-Sheet Fabrication Replaces Rotational Moulding for Rectangular Chemical Process Tanks

    When rectangular chemical process tanks are fabricated from extruded HMS100 sheets instead of rotomoulded polyethylene, the resin is first extruded into 10–25 mm thick sheets on a single-screw extruder with a 30:1 L/D barrier screw, at a melt temperature of 200–220°C, then rough-planed with a carbide-tipped router to remove surface oxidation before welding. The sheet formulation is 100 phr HMS100, with 0.05–0.1 phr processing stabilizer and no mineral filler; welding rod is produced from the same resin batch to avoid melt-flow mismatch at the fusion interface. Panel joining is performed by hot-gas extrusion welding at 210–230°C with a 4–5 mm weld shoe at a travel speed of 250–400 mm/min, and by heated-tool butt fusion at 200–220°C with a bead-up pressure of 0.15 ± 0.03 MPa. Weld tensile performance is validated by ISO 13953:2001, and the finished tank undergoes a 24-hour hydrostatic test at 110% of service pressure. Compliance for stationary welded tanks refers to DVS 2207-1 for hot-gas welding and DVS 2203-4 for penetrant testing; chemical resistance is confirmed by immersion testing per ISO 175:2010 against the stored electrolyte or etchant. A notable fabrication boundary is that weld protrusion above 3 mm on the internal wall creates crevices where chloride solutions accumulate; grinding the weld bead flush is mandatory for electroplating service. Terminal product forms include rectangular electroplating process tanks, chemical etch tanks for aluminium conversion coating, secondary containment trays, and axial ventilation ductwork for acid-exhaust systems.

    Free Quote

    Competitive Tosoh HDPE HMS100 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Tosoh HDPE HMS100 is a high-molecular-weight high-density polyethylene supplied by Tosoh Corporation for extrusion blow moulding of large-volume containers, automotive fuel tanks, intermediate bulk containers, and thick-walled industrial packaging. The grade designation HMS100 identifies a high-molecular-weight structure with controlled density for slow crack growth resistance. Nominal density is 0.954 g/cm³ when measured under ISO 1183-1:2019. Melt mass-flow rate at 190 °C and 2.16 kg is 0.10 g/10 min, while high-load melt flow rate at 190 °C and 21.6 kg is 10.0 g/10 min under ISO 1133-1:2022. The resulting flow-rate ratio near 100:1 is an indirect marker of broad molecular weight distribution and pronounced shear thinning, but it does not replace direct capillary rheometry or extensional viscosity measurement for tooling design.

    PropertyTest methodUnitRepresentative value
    DensityISO 1183-1:2019g/cm³0.954
    Melt mass-flow rate, 190 °C/2.16 kgISO 1133-1:2022g/10 min0.10
    High-load melt flow rate, 190 °C/21.6 kgISO 1133-1:2022g/10 min10.0
    Tensile stress at yieldISO 527-2:2012MPa26
    Tensile elongation at breakISO 527-2:2012%>800
    Flexural modulusISO 178:2019MPa1,100
    Notched Charpy impact, 23 °CISO 179-1/1eA:2010kJ/m²No break
    Notched Charpy impact, −40 °CISO 179-1/1eA:2010kJ/m²12
    Vicat softening temperature, A120ISO 306:2013°C126
    Shore D hardnessISO 868:2003—65
    Environmental stress crack resistance, F50, 100 % Igepal CO-630, 50 °CASTM D1693-15h>1,000

    The listed values are representative of compression-moulded plaques prepared under ISO 1872-2 and are not batch release minima. On production lots, flexural modulus can vary by ±40 MPa and notched Charpy impact at −40 °C can vary by ±4 kJ/m² due to normal molecular weight distribution shift. For load-bearing applications requiring minimum values, a lot-specific certificate of analysis should be requested.

    Compared with a typical injection moulding HDPE having a melt mass-flow rate of 0.30–0.80 g/10 min, HMS100 sacrifices ease of thin-wall mould filling and cycle time but provides substantially higher environmental stress crack resistance and greater parison hang strength. The difference is most pronounced in thick-section blow moulded parts where wall thickness is above 4 mm and service temperature can fall below −20 °C.

    What Limits the Extrusion Blow Moulding Processing Window?

    In accumulator-head shuttle machines with grooved-feed extruders of 90–120 mm diameter and L/D 24–30, the practical melt temperature band is 195–215 °C. Below 190 °C, sharkskin melt fracture on the outer parison surface and die-lip deposit increase sharply, while above 215 °C parison sag becomes the rate-limiting defect for containers with shot volume greater than 200 L. Die gap settings of 2.5–5.0 mm and parison swell between 20 % and 35 % are typical on continuous extrusion lines, but accumulator-head machines require longer parison dwell times and more aggressive parison programming to compensate for diameter swell.

    Clamp force settings of 80–150 t for 220 L open-head drums provide adequate pinch-off weld pressure. Pinch-off weld failure has been observed when clamp force falls below 0.5 t per linear cm of weld length or when mould temperature drops below 10 °C, because the high-molecular-weight tail slows interdiffusion across the weld interface. Cooling time for 5–8 mm wall sections is generally 180–300 s at mould temperatures of 15–25 °C. Demoulding before the internal surface temperature falls below 70 °C can produce post-mould warpage and dimensional instability.

    Pre-drying is not required for pellets stored in sealed packaging below 60 % relative humidity. If condensation is present or surface moisture exceeds 0.05 wt%, drying at 70–80 °C for 4 h in a desiccant hopper is recommended. Barrel temperature profiles may be reverse or flat: feed zone 180–190 °C, compression 190–200 °C, metering 195–205 °C, head and accumulator 195–210 °C. High-shear mixing sections can raise melt temperature by 3–8 °C at screw speeds of 50–80 rpm.

    On accumulator-head machines with a 120 mm extruder, a typical final die gap taper from 4.0 mm to 2.8 mm reduces top-to-bottom wall thinning in a 1.8 m parison. At a melt temperature of 205 °C, parison hang time should not exceed 12 s for a 220 L drum parison before mould closing. Beyond that time, lower parison section thinning can exceed 15 % and reduce drop impact performance. Blow pressure of 0.6–0.9 MPa is typical for thick-walled containers. Mould vents with a depth of 0.02–0.04 mm prevent trapped air at the bottom radius; vent clogging can cause local thinning and parison blowouts.

    Slow Crack Growth, Chemical Resistance, and ESCR Hierarchy

    The high environmental stress crack resistance of HMS100 is most relevant to moulded parts exposed to polar organic liquids, surfactant solutions, and non-oxidising acids at ambient to 60 °C. Under ASTM D1693-15 with 100 % Igepal CO-630, F50 values above 1,000 h are typical for compression-moulded plaques. This places the grade in the high-ESCR segment of HDPE blow moulding resins, distinct from standard unimodal HDPE grades that commonly fail before 200 h under the same test condition.

    However, environmental stress crack resistance is not equivalent to chemical resistance. Concentrated oxidising acids, halogens, and aromatic hydrocarbons can still soften or stress-crack the surface. For fuel tank service, permeation resistance must be assessed by the specific automotive requirement, not by density alone. Published data for this specific configuration is limited, and tank-level fuel permeation testing under 40 CFR 86 or an equivalent procedure should be conducted before production release.

    For hot-water or outdoor service, oxidative stability should be evaluated by oxidation induction time under ISO 11357-6:2018. Published data for this specific grade is limited, so processors should establish a minimum acceptable value for the intended service temperature and antioxidant package. Long-term pressure-pipe classification cannot be inferred from resin density and MFR data alone. A pipe compound must meet the hydrostatic failure knees in ISO 9080:2012 and the classification rules of ISO 12162-1 before being designated PE100 or another pressure class.

    In solid-wall pipe extrusion, the high melt strength of HMS100 stabilises annular flow and reduces sag in large-diameter thick-wall parisons, but pipe-grade certification remains application-specific. Processors should not substitute HMS100 into pressure-pipe applications without completed pipe-compound qualifications.

    When Sub-Zero Impact Resistance Governs Drum and IBC Design

    Large blow moulded containers for cold-climate transport experience impact at temperatures below −20 °C. The notched Charpy impact value at −40 °C of 12 kJ/m² under ISO 179-1/1eA:2010 indicates sufficient low-temperature crack initiation resistance for many thick-walled drum applications, but actual drop impact performance depends on pinch-off weld quality, wall thickness distribution, and the presence of internal knit lines. Drop impact testing on finished containers should be performed at the specified service temperature, typically −18 °C or −29 °C, using the applicable dangerous goods protocol where required.

    The differentiation from Tosoh’s lower-molecular-weight HDPE film and injection grades is most apparent in melt strength and environmental stress crack resistance. However, HMS100 is not suitable for cast film lines designed for 0.5 g/10 min melt-flow resins because bubble stability is inadequate at high throughput. The choice between HMS100 and lower-molecular-weight HDPE is therefore driven by the stress-cracking environment and part geometry rather than by density alone.

    Where outdoor storage is specified, natural HMS100 should not be used without a carbon black masterbatch or UV stabiliser package. The typical addition is 2.0–2.5 wt% carbon black with dispersion assessed under ISO 21870:2004. Excessive external lubricants or silicone-based mould release sprays can migrate into the pinch-off zone and reduce weld factor below 0.80 relative to the adjacent wall.

    Regulatory domainStandard or regulationClause or test methodTypical position for HMS100
    EU food contactRegulation (EU) 10/2011Overall migration via EN 1186Grade-specific compliance certification required
    US food contactFDA 21 CFR 177.1520Olefin polymersGrade-specific compliance certification required
    RoHS heavy metalsDirective 2011/65/EUAnnex IINot intentionally added; supplier declaration required
    REACHRegulation (EC) No 1907/2006Article 33No SVHC above threshold on supplier SDS
    UV-stabilised outdoor serviceISO 21870:2004Carbon black dispersion2.0–2.5 wt% carbon black recommended if not pre-compounded

    Each lot should be traceable to the supplier certificate of analysis. Without lot-level data, designing to minimum values is not permitted for dangerous goods packaging or other safety-critical blow moulded containers. The most conservative approach is to validate the actual container on the production line using the specific mould, accumulator-head machine, regrind ratio, and wall thickness programme intended for serial production.