Tosoh Hdpe D600

Tosoh HDPE D600

    VTB
    Specifications
    HS Code 617460
    Material Type High Density Polyethylene (HDPE)
    Density 0.960 g/cm3
    Melt Flow Rate 190 C 2 16 Kg 0.05 g/10 min
    Tensile Strength At Yield 30 MPa
    Tensile Strength At Break 30 MPa
    Elongation At Break 500%
    Flexural Modulus 1300 MPa
    Notched Izod Impact Strength 200 J/m
    Shore D Hardness 65
    Vicat Softening Temperature 128°C
    Melting Temperature 136°C
    Brittleness Temperature -70°C
    Environmental Stress Crack Resistance >1000 h
    Water Absorption 0.010%
    Volume Resistivity 1e17 ohm-cm
    Dielectric Constant 2.30
    Dissipation Factor 0.00020

    As an accredited Tosoh HDPE D600 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Tosoh HDPE D600 is supplied in 25 kg bags, 40 bags per pallet (1,000 kg), or 1,000 kg bulk bags.
    Container Loading (20′ FCL) Tosoh HDPE D600 resin loaded in a 20-foot FCL container, palletized bags, securely stowed for standard dry ocean shipment.
    Shipping Tosoh HDPE D600 is a non-hazardous, solid high-density polyethylene resin. It is not regulated for transport by DOT, IMDG, IATA, or ADR. Ship in sealed bags, boxes, or bulk containers. Protect from moisture, contamination, and excessive heat. Use standard freight; avoid dust generation and static discharge. No hazardous labels required.
    Storage Store Tosoh HDPE D600 in a cool, dry, well-ventilated warehouse. Keep original containers closed and palletized, away from direct sunlight, heat, ignition sources, moisture, and strong oxidizers. Avoid prolonged UV exposure and extreme temperatures. Maintain clean handling areas to prevent contamination and static buildup. Follow manufacturer’s recommendations and local regulations. Do not stack beyond safe limits. Use first-in, first-out stock rotation.
    Shelf Life Tosoh HDPE D600 typically has a 24-month shelf life if kept in original packaging, cool, dry, and away from sunlight.
    Application of Tosoh HDPE D600

    Reciprocating-screw blow moulding of 120 L to 220 L open-head and tight-head drums with Tosoh HDPE D600 on a 90 mm grooved-feed extruder (L/D 30:1) and a first-in first-out accumulator head requires barrel set temperatures of 180 °C, 190 °C, 205 °C, 205 °C, and accumulator head tooling at 200 °C, with die-exit melt temperature held within 195 °C to 210 °C. The diverging parison die has an adjustable gap of 1.2 mm to 2.5 mm; parison programming is performed in 10 to 25 segments depending on the accumulator head controller, with the lower segment weight increased by 8% to 15% relative to the upper segment to compensate for parison sag. Pre-blow pressure is set at 0.2 MPa to 0.4 MPa and final blow pressure at 0.7 MPa to 0.9 MPa; mould cooling water is supplied at 8 °C to 15 °C to obtain a solidified wall temperature below 80 °C before demoulding, which prevents handle pinching and bottom flash tearing. Where the finished container is intended for direct food contact, the blended formulation must comply with 21 CFR 177.1520(c) specifications for olefin homopolymers and EU 10/2011 overall migration limit of 10 mg/dm²; compliance is not an inherent property of D600 alone but a function of the complete additive package, masterbatch carrier, and processing stabiliser retention, so extraction testing under EN 1186 is required for each production campaign. For dangerous-goods packagings tested as UN 1H1 or 1H2, drop and stacking performance must be revalidated whenever regrind content exceeds 20% by weight because variable molecular-weight distribution from recycled process scrap alters environmental stress crack resistance measured under ASTM D1693 condition B. Dry-air hopper conditioning is not normally required at ambient relative humidity below 50%; above that threshold, condensed surface moisture on cold pellets causes feed-throat slip, melt-pressure oscillation, and intermittent parison length variation, and a dehumidified hopper sweep with dew point below -20 °C is recommended. Published data for this specific accumulator-head configuration on D600 is limited; start-up should therefore begin at the lower parison-weight setting and increase in 2% increments while monitoring die swell and container wall-thickness distribution.

    Why does frost-line height shift during 18 µm blown film production?

    The frost-line shift observed when a 65 mm single-screw extruder with a barrier screw at compression ratio 2.8:1 and a 250 mm spiral mandrel die with 0.8 mm die gap produces 18 µm film is caused by the increased specific output per unit film thickness. For a 20 µm to 25 µm D600 film, the frost-line height is typically stable at 650 mm to 850 mm at a blow-up ratio of 3.5:1; at 18 µm, the lower melt mass per unit area cools more rapidly and the frost line must be lowered to 500 mm to 600 mm to avoid full solidification below the upper collapsing frame, which produces wrinkling and gauge bands. Cooling-ring air velocity is set between 1.5 m/s and 3.0 m/s, with lower-lip air biased against the rotating direction of the bubble to counteract helical instability at blow-up ratios above 4.0:1. Die-exit melt temperature is maintained between 195 °C and 210 °C; below 185 °C, high-molecular-weight D600 generates elevated die pressure and sharkskin on the inner bubble surface, while above 220 °C, melt strength drops enough to cause bubble oscillation and oxidation-induced gel accumulation on the die lips. Terminal products include frozen-food liners, cereal box liners, and heavy-duty sacks where puncture resistance is required. Direct food-contact film uses 21 CFR 177.1520 and EU 10/2011 as the governing frameworks, but migration testing under EN 1186 must be performed on the finished film because printing substrates and surface inks introduce low-molecular-weight migrants that are not present in unstabilised D600 pellets. Process scrap re-incorporation is limited to 15% by weight for films below 20 µm; higher recycled content shifts molecular-weight distribution and destabilises bubble tension, requiring an additional 10% reduction in frost-line height.

    Sheet gauge variation before heavy-gauge thermoforming

    A 120 mm single-screw extruder with barrier screw, melt pump, and flexible-lip coat-hanger die running 1.0 mm to 2.5 mm D600 sheet requires melt-pump inlet pressure of 5 MPa to 8 MPa and die lip opening set 0.1 mm to 0.2 mm above target sheet gauge to compensate for die swell. The vertical three-roll polishing stack is run with lower-roll temperature at 70 °C, middle-roll temperature at 80 °C, and upper-roll temperature at 85 °C; roll gap is set 0.05 mm below target gauge to provide compaction and surface gloss. A traversing beta gauge holds cross-web thickness to ±0.03 mm across a 2200 mm web; variation beyond this value leads to corner thinning and stress whitening in deep-draw thermoformed trays. Sheet intended for food-contact thermoforming must satisfy EU 10/2011 overall migration and 21 CFR 177.1520, while industrial sheet for dunnage and pallet lids is screened under REACH Annex XVII restrictions and RoHS Directive 2011/65/EU for lead, mercury, cadmium, and hexavalent chromium. Antistatic or slip masterbatches are added at 1% to 3% by weight; these additives reduce melt strength and require a 5 °C to 8 °C reduction in melt-pump and die temperatures to maintain edge stability. The principal processing conflict is melt-temperature overshoot during throughput changes, which reduces local viscosity and creates centre-gauge thinning; melt-pump speed is therefore ramped in 0.5 rpm/min increments, and die-bolt profile adjustments are made only after the melt pump reaches steady-state inlet pressure.

    Downstream segmentPrimary regulatory instrumentTest methodCritical parameter
    Blow-moulded food-contact liners21 CFR 177.1520, EU 10/2011EN 1186Overall migration 10 mg/dm²
    Blown film for dry foodFDA 21 CFR 177.1520extraction per 21 CFR 177.1520(c)olefin homopolymer identity
    Heavy-gauge sheetREACH Annex XVII, 2011/65/EUXRF screeningrestricted elements below 0.1%
    Drainage pipeEN 13476-3ring stiffness EN ISO 9969declared SN4 or SN8 class
    Injection-moulded cratesEU 10/2011EN 1186migration 10 mg/dm²

    Monoaxial orientation of D600 on a 75 mm single-screw extruder with 24-hole strand die and a 3 m water-quench bath at 30 °C to 40 °C produces semicrystalline monofilaments with a cold draw ratio of 6:1 to 8:1 between first and second godet stands. Quench water temperature is held above 25 °C to prevent brittle skin formation and below 45 °C to prevent strand adhesion; the air gap between die face and water surface is set at 15 mm to 25 mm because a shorter gap traps air bubbles on the filament surface and a longer gap causes uncontrolled ambient cooling and ovality. After the first godet stand, filaments enter a hot-air orientation oven at 110 °C to 120 °C; the second godet stand runs at 6.0 to 8.0 times first-stand speed, and a third stand applies 3% to 5% relaxation at 115 °C to limit shrinkage below 3% after 15 min in water at 80 °C. Terminal products are industrial rope, monofilament netting, and heavy-duty strapping. Compliance for food-contact netting is assessed under 21 CFR 177.1520 and EU 10/2011; for agricultural netting, the dominant regulatory concern is ultraviolet-stabiliser selection under REACH Annex XVII restrictions. Process scrap and off-spec monofilament can be re-pelletised at up to 10% by weight; higher recycled content lowers drawability and causes filament breaks in the hot-air oven because local molecular-weight degradation reduces melt extensibility.

    Vacuum-assisted corrugators expose wall-thickness variation during corrugation forming

    For non-pressure drainage pipe, D600 is extruded on a 90 mm grooved-barrel extruder feeding a pipe head with spider-leg mandrel and a vacuum-assisted mold-block corrugator; barrel zones are set at 190 °C, 200 °C, 210 °C, and 215 °C, die temperature at 205 °C, and die-exit melt temperature is held between 200 °C and 220 °C. Corrugator vacuum is set at 50 kPa to 75 kPa, with additional blowing air at 0.02 MPa to 0.05 MPa to force the parison into the corrugation profile; ultrasonic thickness heads downstream monitor inner liner wall above 0.8 mm for DN/ID 300 mm systems. Wall-thickness variation in the corrugation valleys is the dominant failure mode because thin spots reduce local ring stiffness and create buckling sites under soil load; ring stiffness is tested according to EN ISO 9969 and must meet the declared SN4 or SN8 class of EN 13476-3. D600 without a pressure-pipe carbon-black masterbatch is not qualified for potable-water pressure service; where hydrostatic stress regression is required, testing under ISO 9080 and classification under ISO 12162 must be performed on the specific pigmented compound used in production. Terminal products include agricultural field drainage, road-edge storm-water conduits, and landfill leachate collection pipe. Reprocessed D600 from start-up scrap is added at up to 15% by weight; higher addition rates broaden the molecular-weight distribution and cause inner-wall melt fracture, observed as axial streaks downstream of the corrugator.

    When a 3.5 kg thick-walled crate is injection-moulded at low injection velocity

    Injection moulding of thick-walled industrial containers from D600 is carried out on a reciprocating-screw injection-moulding machine with clamp force determined by cavity pressure and projected area; for a 450 mm × 600 mm pallet base with 4 mm nominal wall thickness, injection speed is set between 20 mm/s and 35 mm/s to prevent jetting and surface splay. Barrel setpoints are 200 °C, 210 °C, 215 °C, 215 °C, and nozzle at 210 °C; mould temperature is controlled at 15 °C to 25 °C. Hold pressure is 60 MPa to 80 MPa for 10 s to 15 s, screw back pressure 0.5 MPa to 0.8 MPa, screw speed 35 rpm to 50 rpm, cushion 3 mm to 6 mm, and cooling time for a 3.5 kg crate is 90 s to 120 s. Demoulding before part surface temperature falls below 75 °C causes corner distortion and post-ejection dimensional recovery. The low-melt-flow character of D600 limits practical flow-length-to-wall-thickness ratio to approximately 120:1; sections thinner than 2.5 mm require multiple drop gates and mould-filling simulation before tool steel release to avoid short shots. Terminal products include returnable transport crates, food-grade bulk bin bases, and tote bins for industrial storage. For food-contact crates, EU 10/2011 overall migration of 10 mg/dm² and 21 CFR 177.1520 apply to the complete formulation, and finished articles must be extraction-tested under EN 1186. Regrind from gates and runners is re-introduced at up to 20% by weight without excessive loss of impact strength measured under ISO 179-1/1eA, but higher regrind content increases shrinkage anisotropy and makes flatness of the pallet base difficult to hold.

    Free Quote

    Competitive Tosoh HDPE D600 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Tosoh HDPE D600 is a high-density polyethylene homopolymer grade distributed within the Tosoh Nipolon HDPE portfolio. The D-series designation places the resin in the extrusion blow moulding and thick-walled sheet tier, with the numeric suffix 600 ordering melt flow rate and density within the producer’s grade ladder. Published English-language certifications for D600 are limited; where a lot-specific certificate of analysis is unavailable, the numerical ranges in this document follow the class envelope for high-density polyethylene homopolymer blow moulding resins measured under ISO 1183-1:2019, ISO 1133-1:2022, ISO 527-2:2012, and ASTM D1693-15.

    How Does the Melt Flow Rate Tier Constrain Extrusion Blow Moulding?

    Melt flow rate is the principal control variable separating D600 from fast-cycle injection moulding high-density polyethylene grades. A melt flow rate of 0.3 g/10 min to 0.7 g/10 min at 190 °C under 2.16 kg load, measured according to ISO 1133-1:2022, indicates high average molecular weight and high low-shear viscosity. On a continuous shuttle blow moulding line using a grooved-feed extruder of 25:1 L/D to 30:1 L/D, this viscosity reduces parison sag and supports accumulator-head programming. Accumulator-head tooling with a diverging die gap of 1.5 mm to 4.0 mm is typically operated at melt temperatures from 180 °C to 220 °C; below 180 °C sharkskin and die-lip fouling increase, while above 220 °C parison sag and oxidative gel formation become more probable. The practical head-temperature window is therefore approximately ±10 °C around the setting selected for a given accumulator volume and part weight.

    Surface moisture on pellets stored below plant dew point can introduce splay and surface pitting in thick-walled parts. Although high-density polyethylene is not hydrolytically sensitive, pellets conditioned at 85 °C for 2 h in a desiccant hopper drier are recommended when warehouse relative humidity exceeds 60% or when regrind content above 20 wt% is reintroduced. Extruder zones are commonly profiled from feed zone 170 °C to head 200 °C, with feed-throat cooling held at 40 °C to 60 °C to prevent pellet bridging. Extruder backpressure is normally kept below 25 MPa; higher backpressure raises residence time and can degrade the high-viscosity melt. Specific D600 trials may require adjustment within ±5 °C of the listed zone settings.

    Density, Crystallinity, and Environmental Stress Crack Resistance

    Density controls crystalline mass fraction and therefore the stiffness and permeation behaviour of the finished wall. The D600 tier is typically specified at 0.955 g/cm³ to 0.962 g/cm³ at 23 °C under ISO 1183-1:2019, corresponding to a crystalline mass fraction of approximately 70% to 78% when referenced to the ideal orthorhombic polyethylene crystalline density. Environmental stress crack resistance is a limiting property in rigid containers exposed to surfactants, agricultural chemicals, or non-solvent oils. The following consolidated property envelope is intended for preliminary engineering comparison and does not replace a certified lot-specific certificate of analysis.

    PropertyTest MethodTypical Envelope
    Melt flow rate (190 °C, 2.16 kg)ISO 1133-1:20220.3–0.7 g/10 min
    Density (23 °C)ISO 1183-1:20190.955–0.962 g/cm³
    Tensile stress at yieldISO 527-2:201228–32 MPa
    Tensile elongation at breakISO 527-2:2012>600%
    Flexural modulusISO 178:20191,300–1,700 MPa
    Charpy notched impact strength (23 °C)ISO 179-1:20106–10 kJ/m²
    Vicat softening temperature (A50)ISO 306:2022125–130 °C
    Environmental stress crack resistance (100% Igepal CO-630, F50)ASTM D1693-15>100 h

    The environmental stress crack resistance threshold of >100 h under ASTM D1693-15 applies to specimens conditioned in nonylphenoxy poly(ethyleneoxy) ethanol solution at 50 °C. Values below 50 h are generally associated with lower molecular weight or broader molecular weight distribution blow moulding grades. Because D600 is a homopolymer rather than a hexene-comonomer-modified high-density copolymer, its resistance to bleach-containing cleaners and polar surfactants is lower than that of bimodal or octene-comonomer grades. For aggressive agricultural chemical packaging, published comparative data for this specific configuration is limited; qualification should include finished-container burst testing under ASTM D2561 or equivalent pack performance protocols, not resin-level environmental stress crack resistance alone.

    When D600 Replaces General-Purpose HDPE in Thick-Walled Container Production

    When D600 is evaluated as a drop-in replacement for a general-purpose high-flow high-density polyethylene in thick-walled container production, cycle time and pressure demand change because the lower melt flow rate increases resistance to flow. On an injection moulding machine with clamp force below 2,500 kN, wall sections above 4 mm can develop sink marks and elevated cavity-pressure requirements. In extrusion blow moulding, the lower melt flow rate shifts the process window toward longer parison hang time and reduced die-gap dependence. At equal wall thickness, a density in the 0.955–0.962 g/cm³ bracket is higher by 0.010–0.017 g/cm³ than a typical 0.945 g/cm³ general-purpose high-density polyethylene; top-load performance should be confirmed by ASTM D2659 column crush testing on the finished article because geometry and wall distribution dominate the final result.

    For extrusion blow moulding of containers with wall thickness above 3 mm, mould temperature is normally held at 10 °C to 30 °C using turbulent-flow water circuits. Cooling time scales approximately with the square of wall thickness; increasing wall thickness from 3 mm to 5 mm can increase cycle time by a factor of 2.0–2.8 when all other variables are fixed. Excessively high blow pressure above 0.6 MPa can distort parison layflat and produce folded seams. A target blow pressure of 0.45–0.60 MPa is commonly set for this viscosity tier, with profile adjustments made through wall-thickness sensor feedback.

    Differentiating the D-Series Grade Ladder and Substitution Boundaries

    The most frequent substitution error occurs when a converter assumes all high-density polyethylene grades within the same density band are interchangeable. The D-series grade ladder is not a single-variable melt flow rate progression; molecular weight distribution, stabiliser package, and polymer architecture alter processing and end-use performance. Published data for D600-specific molecular weight distribution curves are limited. The following comparative matrix is therefore constructed from class-typical behaviours, not from direct Tosoh certification.

    ParameterD600 TierHigh-Flow Injection HDPEBimodal Pipe HDPE
    Melt flow rate (190 °C, 2.16 kg)0.3–0.7 g/10 min8–40 g/10 min0.2–0.5 g/10 min
    Density0.955–0.962 g/cm³0.950–0.960 g/cm³0.948–0.960 g/cm³
    Primary conversion routeExtrusion blow mouldingInjection mouldingPipe extrusion
    Melt strengthHighLowVery high
    Environmental stress crack resistanceModerateLow to moderateHigh
    Molecular architectureUnimodal, narrower molecular weight distributionControlled rheologyBimodal

    A direct substitution into a pipe extrusion line is not appropriate for D600 if the pipe is classified under ISO 9080 long-term hydrostatic strength requirements. D600 belongs to the blow moulding tier, not the PE100 or PE100-RC pipe grade tier. Incoming inspection for food-contact or high-pressure container applications should include gel count per ISO 18553:2002, oxidation induction time by ISO 11357-6:2018, and ash content by ISO 3451-1:2019. Compliance under FDA 21 CFR 177.1520 should be verified against the specific lot certificate, because olefin polymer clearances are composition-dependent and are not automatically granted by polymer type alone. REACH and RoHS compliance for D600 should be confirmed through the supplier safety data sheet and product stewardship declaration. Polyethylene homopolymer grades generally contain phenolic antioxidant and phosphite stabiliser packages; migration limits under EU Regulation 10/2011 depend on overall and specific migration testing of the finished article. No statement in this introduction replaces a migration certificate for food-contact use.

    Top