| HS Code | 470119 |
| Grade | Toraycon 1401X06 |
| Polymertype | PBT |
| Reinforcement | Unreinforced |
| Moldshrinkage Percent | 1.5-2.0 |
| Processingtemperature C | 240-260 |
| Dryingtime H | 3-4 |
| Volumeresistivity Ohm Cm | 1E16 |
As an accredited Toray Toraycon® Unreinforced PBT 1401X06 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Toray Toraycon® Unreinforced PBT 1401X06 is supplied in 25 kg moisture-resistant bags for safe handling, storage, and transport. |
| Container Loading (20′ FCL) | For 20′ FCL loading, Toray Toraycon® Unreinforced PBT 1401X06 is packed in moisture-proof bags on pallets, securely stowed and braced for ocean transport. |
| Shipping | Toray Toraycon® Unreinforced PBT 1401X06 is shipped as dry resin pellets in sealed moisture-barrier bags or containers, palletized and protected from weather. It is non-hazardous for transport, should be kept cool and dry, and handled to avoid contamination or package damage. Standard freight; refer to SDS and local regulations. |
| Storage | Store Toray Toraycon® Unreinforced PBT 1401X06 in a cool, dry, well-ventilated area away from direct sunlight, heat, and ignition sources. Keep containers tightly closed to prevent moisture absorption and contamination. Avoid contact with strong oxidizers. Follow first-in, first-out stock rotation, and dry/condition material per supplier recommendations before processing if exposed to humid conditions. |
| Shelf Life | Shelf life is approximately two years when stored unopened in original packaging in a cool, dry place, protected from sunlight. |
Competitive Toray Toraycon® Unreinforced PBT 1401X06 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Toray Toraycon® Unreinforced PBT 1401X06 is an unfilled polybutylene terephthalate injection-molding resin supplied by Toray Industries, Inc. The grade is characterized by a non-fibrous, single-phase matrix and a flame-retardant additive system. Under the vertical burn classification of UL 94, this product is commonly rated V-0 at a nominal thickness of 0.8 mm; certification must be verified in the final color and wall thickness. The notation “unreinforced” distinguishes this material from glass-fiber and mineral-filled PBT compounds that exhibit higher flexural modulus, lower mold shrinkage, and greater anisotropy. The principal processing route is injection molding, and the grade is typically specified for relay bases, coil bobbins, switch housings, connector bodies, and thin-wall electrical insulation parts. The material is not intended for continuous structural load bearing above the limits of unfilled PBT, nor for blow molding or blown film extrusion unless process-specific rheology is validated against production equipment.
Table 1 consolidates representative values from published manufacturer literature. These values are typical ranges and should not be used as batch release limits without reviewing a production lot certificate.
| Property | Test method | Unit | Representative value |
|---|---|---|---|
| Specific gravity | ASTM D792-20 | — | 1.43–1.46 |
| Water absorption, 24 h | ASTM D570-98 | % | 0.06–0.08 |
| Tensile strength at break | ASTM D638-14, Type I | MPa | 52–58 |
| Tensile elongation at break | ASTM D638-14 | % | 20–30 |
| Flexural strength | ASTM D790-17 | MPa | 80–90 |
| Flexural modulus | ASTM D790-17 | GPa | 2.3–2.5 |
| Notched Izod impact at 23 °C | ASTM D256-10 | J/m | 40–50 |
| Heat deflection temperature at 1.80 MPa | ASTM D648-18 | °C | 55–65 |
| Flammability rating at 0.8 mm | UL 94 | — | V-0 |
| Volume resistivity | ASTM D257-14 | Ω·cm | 1.0 × 10^15 |
| Dielectric strength, short-time | ASTM D149-20 | kV/mm | 16–20 |
| Mold shrinkage, flow direction | ASTM D955-08 | % | 1.5–2.0 |
Under ISO 75-1/2, unfilled flame-retardant PBT of this class exhibits heat deflection temperature at 1.80 MPa near 60 °C. In contrast, published data for 30 wt% short-glass PBT compounds indicate HDT/A values exceeding 200 °C under the same stress. The mechanism is direct: glass fiber restricts the cooperative movement of amorphous chain segments. The lower HDT of 1401X06 means it is not selected for load-bearing parts in hot zones above 80 °C unless support geometry compensates. However, the unreinforced material produces nearly isotropic shrinkage; representative mold shrinkage is 1.5–2.0% in flow and transverse axes, while glass-filled PBT may show 0.2–0.6% flow-direction and 0.8–1.2% transverse-direction shrinkage. The resulting differential shrinkage in glass-filled grades creates warpage in flat connector bodies, bobbins, and cover housings, forcing additional cooling-channel adjustments or fixturing after demolding.
Comparing 1401X06 with unmodified PBT, the flame-retardant system increases specific gravity from approximately 1.31 g/cm³ to 1.43–1.46 g/cm³ under ASTM D792-20. This changes melt density and shot-volume calculations because a denser melt delivers higher cavity pressure for the same volumetric fill. The flame-retardant additives also modify melt stability; the residence-time window before visible yellowing or black speck formation narrows. In a production setting using an 80-ton toggle-clamp machine with a 20 mm screw, barrel residence time during idle cycles should not exceed 5 min at 250 °C. Published data for this specific configuration is limited, so each molder should establish lot-specific residence limits by measuring tensile strength retention after 10, 20, and 30 idle cycles.
Mineral-filled flame-retardant PBT grades typically develop lower notched impact strength and higher flexural modulus than unreinforced 1401X06. While 1401X06 lists notched Izod impact near 45 J/m, mineral-filled grades may fall below 30 J/m while increasing flexural modulus above 3.0 GPa. If the part requires snap-fit deflection, the unreinforced grade is preferred; if the part must hold tight tolerances over a broad temperature range, a mineral-filled or glass-filled grade is preferred because the coefficient of linear thermal expansion is lower. The unreinforced grade also offers elongation at break of 20–30%, allowing limited post-mold insertion of metal pins without fracture at the insertion site.
Rheological behavior of unreinforced 1401X06 is pseudoplastic and strongly shear-rate dependent. In capillary rheometry under ISO 11443:2021 at 250 °C, unfilled PBT grades of similar molecular architecture typically show apparent viscosity decreasing from roughly 70–100 Pa·s at 100 s⁻¹ to 20–40 Pa·s at 1,000 s⁻¹; grade-specific data should be obtained from the lot certificate because additive type affects shear sensitivity. The rapid crystallization of PBT limits the low-viscosity flow window. The melt begins to solidify near 190 °C, so thin-wall filling below 0.5 mm requires high injection speed and valveless hot-runner tips to avoid premature freeze-off. Cold-runner gates for this grade are generally dimensioned at 50–70% of the adjacent wall thickness; a gate land length greater than 0.8 mm can cause pressure loss and jetting on the cavity surface. Vent depths of 0.012–0.025 mm are set along the flow path because trapped air and volatile flame-retardant decomposition products produce burn marks and deposit buildup on vents.
On a production-scale reciprocating-screw injection molding machine, a general-purpose screw with L/D of at least 18:1 and a low-compression ratio is preferred; a barrier screw may generate excessive shear heating in the feed zone if the pellet softening point is exceeded too early. The material is dried in a desiccant dryer to 0.02% moisture or less. Drying at 120–130 °C for 3–4 h with a return-air dew point of -30 °C or lower is standard. Wet pellets produce splay, hydrolytic molecular weight loss, and a reduction in tensile strength; grade-specific published data for this moisture condition is limited. The barrel temperature profile is set from 240 °C at the rear zone to 260 °C at the nozzle; sustained melt temperatures above 270 °C accelerate flame-retardant decomposition and can produce plate-out on mold surfaces. Mold temperature is maintained at 40–80 °C. The upper half of this range is used when sprue sticking, gate blush, or post-mold dimensional drift is observed. Back pressure is limited to 0.3–0.7 MPa to avoid shear heating. Because the volumetric shrinkage is 1.5–2.0%, packing pressure must be maintained until gate freeze; premature packing release produces sink marks opposite thick bosses and depressions on flat ribs. Regrind use requires drying and lot-level UL verification because the flame-retardant concentration is sensitive to repeated heat history.
Electrical insulation performance is evaluated under ASTM D257-14 and ASTM D149-20. Published data for this grade list volume resistivity near 1.0 × 10^15 Ω·cm and short-time dielectric strength near 18 kV/mm; both values are thickness- and humidity-dependent and should not be used as dielectric design limits without safety margin. UL Recognized Component certification is typically available for UL 94 V-0 at 0.8 mm, but the final color concentrate, regrind level, and wall thickness can alter the rating. The UL Yellow Card for the specific compound and color must be consulted before production release because orange, red, or white pigment loadings can influence the burn rating at marginal thicknesses.
RoHS compliance is assessed under Directive 2011/65/EU Annex II. RoHS does not automatically prohibit all halogenated flame-retardant chemistries; it restricts defined substances such as polybrominated biphenyls and certain brominated diphenyl ethers. REACH documentation under Regulation (EC) No 1907/2006 must be obtained from the resin supplier for substances of very high concern. The material may not be suitable for food-contact use unless a specific migration test under EU 10/2011 or FDA 21 CFR demonstrates compliance; published data for this specific configuration is limited. For electrical insulating parts, comparative tracking index testing under IEC 60112:2020 should be performed if the part is exposed to surface contamination, because flame-retardant additives can lower tracking resistance relative to unmodified PBT.
Tooling for thin-wall connector housings with nominal wall sections below 1.0 mm should use direct or tunnel gating with short land lengths because the rapid crystallization of PBT reduces flow length in long, unheated cold runners. The melt temperature should be set at 250–260 °C for thin-wall filling; the mold temperature should be held at 60–80 °C to keep the cavity surface above the glass transition of approximately 45–60 °C for unfilled PBT, thereby limiting premature crystallization. Excessively high injection velocity can generate shear heating above 270 °C at the gate and trigger flame-retardant degradation streaks. When insert-molded copper alloy terminals are present, the maximum barrel residence time should be reduced and production interruptions limited because copper ions catalyze thermo-oxidative chain scission. The user should validate tensile strength after 500 h of hot-air aging at 150 °C or after 1,000 h at 85 °C/85% RH using ISO 527-2 specimens, because published lot-specific aging data for 1401X06 may not cover the exact insert configuration.
On an electric connector production line with clamp force below 300 kN, filling imbalance across multi-cavity tools is a known failure mode. The low melt viscosity of unfilled PBT can cause preferential filling of the shortest cavity and underpacking of the farthest cavity. To compensate, the runner system should be balanced to within 5% of the pressure drop between cavities; otherwise flash appears on the near-cavity parting line while the far cavity exhibits sink marks. In-mold labeling or pad printing should be tested after 24 h because flame-retardant additive migration can reduce ink adhesion.
Toraycon® 1401X06 has an operational boundary in hot, humid environments. PBT is hydrolytically degraded by water at temperatures above 60 °C under pressure; long-term exposure to hot-water extraction or autoclave sterilization reduces molecular weight even if the part is not under stress. Chemical incompatibility includes concentrated mineral acids, oxidizing acids, ketones, chlorinated solvents, and strongly alkaline solutions at elevated temperature. Stress-cracking agents include some aromatic hydrocarbons and aliphatic halides. The grade should not be processed in equipment contaminated with polycarbonate or PET at high barrel temperatures because transesterification can shift crystallization and degrade mechanical toughness. For parts used in outdoor enclosures, carbon black or UV-stabilized versions may be required; the unfilled flame-retardant grade itself is not automatically UV-weatherable, and ISO 4892-2 or ASTM D2565-23 exposure data should be generated for the intended color and surface texture. The product is typically supplied in pellet form in moisture-barrier packaging; opened bags should be resealed and re-dried before molding if ambient relative humidity exceeds 60% for more than 4 h.