| HS Code | 786326 |
| Density | 1.35 g/cm³ |
| Water Absorption 23 C 24 H | 0.08% |
| Mold Shrinkage Md | 1.3% |
| Mold Shrinkage Td | 1.6% |
| Tensile Strength | 60 MPa |
| Elongation At Break | 20% |
| Flexural Modulus | 2500 MPa |
| Flexural Strength | 90 MPa |
| Charpy Notched Impact Strength 23 C | 3 kJ/m² |
| Hdt At 1 82 Mpa | 70 °C |
| Hdt At 0 45 Mpa | 150 °C |
| Melting Point | 225 °C |
| Flammability Rating | UL94 V-0 (0.4 mm) |
As an accredited Toray Toraycon® Unreinforced FR PBT 1494X02 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Toray Toraycon® Unreinforced FR PBT 1494X02 is supplied in 25 kg polyethylene-lined paper bags, palletized for industrial handling. |
| Container Loading (20′ FCL) | Toray Toraycon® Unreinforced FR PBT 1494X02 is palletized and securely loaded into a 20′ FCL container under dry, clean conditions. |
| Shipping | Toray Toraycon® Unreinforced FR PBT 1494X02 is shipped as non-hazardous thermoplastic resin pellets in sealed moisture-barrier packaging. It is not regulated for transport under DOT, IMDG, or IATA; no UN number applies. Store cool and dry, away from ignition sources, protecting from moisture and physical damage. |
| Storage | Store Toray Toraycon® Unreinforced FR PBT 1494X02 in a cool, dry, well-ventilated area away from direct sunlight, heat, ignition sources, and oxidizing agents. Keep containers tightly closed to prevent moisture absorption and contamination. Avoid prolonged exposure to humid air. Use first-in, first-out stock rotation. Inspect containers. Follow local regulations and the manufacturer’s safety data sheet for safe handling and storage. |
| Shelf Life | Toray Toraycon® Unreinforced FR PBT 1494X02 typically has a 24-month shelf life when stored dry, cool, and in unopened original packaging. |
Competitive Toray Toraycon® Unreinforced FR PBT 1494X02 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Toray Toraycon® Unreinforced FR PBT 1494X02 is a non-reinforced, flame-retardant polybutylene terephthalate injection-moulding compound supplied in pellet form for electrical insulation and electronic component applications. The grade is formulated around an unfilled PBT backbone combined with a flame-retardant package; no glass fibre or mineral reinforcement is present. This composition retains melt flow for thin-wall connector geometries, but it establishes a mechanical property envelope lower in stiffness and strength than reinforced flame-retardant PBT grades. The material is positioned for parts requiring a UL 94 V-0 flammability classification at the manufacturer’s listed minimum wall thickness, combined with predictable mould shrinkage and resistance to automotive and industrial electrical contaminants.
Grade-specific property values for 1494X02 should be taken from the current Toraycon technical data sheet. Published public data for this exact formulation are limited to the manufacturer’s datasheet; the class envelopes cited below represent unreinforced flame-retardant PBT systems and are not acceptance limits for lot release unless confirmed against the product specification.
Drying before melt processing is required to prevent hydrolytic chain scission. A dehumidifying hopper dryer set at 120 °C for 3–5 h typically lowers residual moisture below 0.02 % by weight. PBT resins hydrolyse at melt temperatures; accumulated moisture converts condensation polymer linkages into lower-molecular-weight fragments, reducing melt viscosity and causing surface streaking, gas burns, and loss of impact strength. The problem is observed on injection lines when wet regrind is blended into virgin pellets without independent drying. Unreinforced flame-retardant PBT grades should not be processed directly from octobin storage if ambient relative humidity exceeds 60 %.
Barrel temperature settings for unfilled FR PBT are commonly profiled from 240 °C at the rear zone to 265–270 °C at the front and nozzle. A nozzle setting of 250–260 °C prevents premature freeze-off at the sprue bushing while limiting residence time at degradation temperature. Mould temperature is maintained between 40 °C and 80 °C; higher mould temperatures within this range produce more complete crystallisation, lower post-mould shrinkage, and more reproducible surface finish at the expense of longer cycle time. Lower mould temperatures shorten cycle time but can produce under-crystallised skins that continue to shrink after ejection. For thin-wall connector housings below 0.8 mm nominal wall, gate thickness and gate freeze time control packing more than barrel temperature because the unfilled melt freezes rapidly. Generous venting is necessary because the flame-retardant package can generate volatiles that cause gas trapping at the flow front.
Compared with non-flame-retardant unreinforced PBT grades, 1494X02 incorporates a flame-retardant system that shifts the flammability rating from the HB class to V-0 at the manufacturer’s listed thickness. The flame-retardant package increases melt density into the class range of 1.42–1.50 g/cm³ measured by ISO 1183-1. Tensile elongation at break is typically reduced relative to unfilled non-FR PBT, while tensile strength remains in the lower half of the unreinforced PBT range. Comparative tracking index may also decline; connector designs with reduced creepage distances should be evaluated by IEC 60112 on moulded plaques to confirm final tracking performance in humid or contaminated field conditions.
Against glass-fibre-reinforced flame-retardant PBT with 30 % glass fibre, the unreinforced grade is significantly lower in tensile strength and flexural modulus. Class data place tensile strength between 45 MPa and 65 MPa for unfilled FR PBT, while PBT GF30 FR typically lies between 110 MPa and 140 MPa under ISO 527-2. Flexural modulus for unfilled FR PBT is approximately 2.4–3.0 GPa, compared with 8.0–10.5 GPa for PBT GF30 FR. The unfilled grade differs by offering more isotropic shrinkage and lower melt viscosity, which can improve filling of thin pin walls and complex core features where glass fibre would cause anisotropic warpage and fibre orientation defects.
Mould shrinkage is the primary tool-design difference. Unreinforced flame-retardant PBT class shrinkage in flow direction ranges from 1.2 % to 2.0 %, while glass-reinforced PBT shrinks at 0.2–0.5 % in the flow direction; the cross-flow shrinkage difference is smaller because glass orientation introduces anisotropy. Tooling for 1494X02 must therefore include larger steel allowances and sufficient draft. Processing parameters such as packing pressure and gate design influence the final shrinkage value, so prototype cavity measurements under production conditions are necessary before hardened steel is cut.
| Property | Test method | Unreinforced FR PBT class | PBT GF30 FR class |
|---|---|---|---|
| Density | ISO 1183-1 | 1.42–1.50 g/cm³ | 1.55–1.70 g/cm³ |
| Tensile strength at break | ISO 527-2 | 45–65 MPa | 110–140 MPa |
| Flexural modulus | ISO 178 | 2.4–3.0 GPa | 8.0–10.5 GPa |
| Charpy notched impact strength | ISO 179-1/1eA | 2–5 kJ/m² | 6–10 kJ/m² |
| Mould shrinkage, flow direction | ISO 294-4 | 1.2–2.0 % | 0.2–0.5 % |
| Heat deflection temperature, 1.82 MPa | ISO 75-1/-2 | 60–80 °C | 200–215 °C |
Specification packages for connectors and relay bodies frequently require verification under UL 94 V-0, IEC 60695-2-11 glow-wire ignition, and IEC 60112 comparative tracking index. The actual flammability classification of 1494X02 is thickness- and colour-dependent; a V-0 listing at 0.75 mm does not automatically extend to 0.4 mm in a different colourant. End-product certification is therefore based on final moulded part thickness and colour masterbatch. For appliance connectors that carry exposed live parts, glow-wire ignition temperature requirements of 750 °C or 850 °C are evaluated according to IEC 60695-2-11; the PBT grade may require design measures such as increased insulation thickness or ceramic inserts if the glow-wire test is exceeded. Comparative tracking index values for flame-retardant PBT are typically lower than non-FR PBT; connector pin spacing must be checked against actual CTI measured on plaques rather than assumed from unfilled non-FR PBT data.
Unreinforced flame-retardant PBT provides predictable insulation resistance in dry and moderately humid electrical environments. Volume resistivity for unfilled PBT generally exceeds 10^13 Ω·m under IEC 60093, and dielectric strength is commonly above 20 kV/mm for thicknesses around 1 mm under IEC 60243-1. These values are class-level; specific 1494X02 values should be confirmed from the manufacturer’s datasheet. Because the material is hygroscopic only to a limited extent, moisture uptake under ISO 62 after 24 h immersion is typically below 0.1 %, which is an order of magnitude lower than polyamide 66. This property reduces dimensional change in humidity cycling and is one reason unfilled PBT is retained for precision coil bobbin flanges.
| Requirement | Standard or test method | Engineering function |
|---|---|---|
| Flammability rating | UL 94 | V-0 at listed minimum thickness; thickness- and colour-dependent |
| Glow-wire ignition | IEC 60695-2-11 | End-product ignition resistance at 750 °C or 850 °C |
| Comparative tracking index | IEC 60112 | Creepage distance validation on moulded plaques |
| Tensile properties | ISO 527-2 | Strength and elongation at break |
| Flexural modulus | ISO 178 | Design stiffness under bending load |
| Impact strength | ISO 179-1/1eA | Notch sensitivity for assembly and service |
| Melt mass-flow rate | ISO 1133-1 | Lot-to-lot processing consistency |
| Mould shrinkage | ISO 294-4 | Tool compensation and dimensional approval |
| Moisture absorption | ISO 62 | Dimensional stability under humidity exposure |
| Restricted substances | 2011/65/EU | RoHS compliance for electrical and electronic equipment |
| Substance evaluation | EC 1907/2006 | REACH SVHC reporting and authorisation |
Flame-retardant packages in PBT may alter melt viscosity. Brominated systems can lower viscosity through synergist effects; halogen-free systems can increase viscosity or narrow the stable processing window. The specific 1494X02 package is not publicly detailed; a moulder should establish a melt flow rate baseline from each lot before drying and compare it against the supplier’s certificate of analysis. Viscosity shifts greater than 10 % can indicate regrind contamination, moisture damage, or incorrect drying history.
Unreinforced flame-retardant PBT freezes sooner than glass-filled PBT and shows a steeper viscosity dependence on shear rate. In hot-runner connector tools, valve-gated drops reduce gate stringing but require sequential opening; unfilled FR PBT can drool from thermal gates if nozzle temperatures exceed 260 °C. If the material is moulded on a multi-cavity tool with more than eight cavities, naturally balanced runner layouts are preferred over geometrically balanced runs, particularly when gate diameters are below 1.0 mm.
Sub-gate freeze-off determines the packing window. If the gate land is too thick, cycle time increases; if too thin, packing pressure is cut off before sink at pin retention bosses can be eliminated. Field experience on injection moulding lines shows that sub-gate diameters between 0.6 mm and 1.0 mm provide a workable starting point for unfilled FR PBT at wall sections between 0.5 mm and 1.5 mm, but published data for this specific configuration are limited. Melt filling studies on the actual tool are required because gate freeze time depends on local part geometry, coolant layout, and flame-retardant package viscosity.
Venting is critical because the flame-retardant package releases limited volatile decomposition products. Vent depths for PBT are normally held below 0.02 mm to avoid flash, but unfilled FR grades may require wider vents at flow-front meeting points to prevent burn marks. Inadequate venting appears as dark streaks at the end of fill, often mistaken for wet resin. If venting is corrected and streaks persist, drying time or residual moisture level should be reviewed before altering barrel temperatures.
Post-mould shrinkage continues for 24–48 h after demoulding. Dimensional approval should therefore be conducted after conditioning, not immediately after ejection. Unreinforced PBT achieves most of its crystallisation shrinkage in the mould, but ambient ageing and moisture uptake produce smaller secondary dimensional changes. Parts destined for precision electrical contact alignment should be measured after conditioning at 23 °C and 50 % relative humidity for at least 24 h, consistent with ISO 291.
Insert moulding introduces additional shrinkage constraints. Cold inserts can cause cracking at the interface because the unfilled polymer has lower crack propagation resistance than glass-filled grades. Insert temperature is typically maintained above mould temperature but below the polymer’s heat-deflection region, often near 80–100 °C. The exact insert temperature depends on insert mass and wall thickness; oversized inserts can act as heat sinks and produce premature freeze, requiring local wall thickening.
The selection of unreinforced flame-retardant PBT over polyphenylene sulfide or glass-fibre-reinforced PBT in a relay base or coil bobbin is driven by a combination of processing temperature, dimensional consistency, and cost. PPS offers higher continuous-use temperature and dimensional stability at reflow temperatures above 260 °C, but it requires barrel temperatures above 300 °C and has a higher melt viscosity. For relay bases exposed to under-hood temperatures below 120 °C, unreinforced FR PBT can avoid the higher tool abrasion and higher material cost associated with PPS while maintaining sufficient insulation. However, if the relay is specified for reflow soldering above 260 °C, PBT is unsuitable because its heat deflection temperature and crystalline melting point are too low.
Compared with glass-filled PBT, the unreinforced grade provides lower anisotropic warpage in flat coil bobbin flanges where glass orientation around the core can cause out-of-flatness. The unfilled material also reduces stress concentration at metal insert interfaces and can accept thin walls more readily. The penalty is lower creep resistance and lower stiffness under winding loads; coil bobbins with high winding tension may require a glass-reinforced flame-retardant PBT or PPS instead. Published comparative data for 1494X02 in this exact application are limited; prototype testing under actual winding tension and terminal insertion force is necessary.
Against thermoset phenolic in relay bases, 1494X02 offers injection-moulding cycle-time advantages and the possibility of regrind reuse. Phenolic requires transfer or compression moulding and generates condensation volatiles; PBT can be processed in fully automatic injection lines with shorter cycles. Phenolic may retain higher heat resistance, but many electrical applications within the PBT thermal envelope select PBT for lower tool maintenance and cleaner moulding surfaces.
Residence time and melt temperature interact to limit the processing window. At barrel settings above 270 °C, increasing melt temperature reduces viscosity only marginally, but the rate of hydrolytic and thermal degradation increases sharply. The degradation products lower molecular weight and deposit on vent and cavity surfaces, producing plate-out and gas burns. Production lines operating with hot-runner manifolds should set hot-runner nozzle temperatures to the lowest value that prevents freeze-off, typically 250–260 °C for unfilled FR PBT. Excessively high hot-runner temperatures cause colour shifts in natural and light-coloured mouldings and can degrade the flame-retardant package, reducing UL 94 V-0 performance.
Regrind usage should be limited and controlled. Unreinforced flame-retardant PBT can be re-ground and blended with virgin resin, but repeated heat history consumes the stabiliser and flame-retardant synergist. A common industrial limit is 20–30 % regrind by weight for electrical components, provided the regrind is dry and free of oil contamination. Higher regrind fractions increase lot-to-lot viscosity variation and may shift shrinkage. For components with UL 94 V-0 certification, regrind levels must not exceed the percentage validated in the material listing and end-product flammability test. The use of regrind from mixed colours or unknown heat history is not recommended.
Hot-water and steam exposure imposes a service boundary. PBT resins are susceptible to hydrolysis at temperatures above 60–80 °C in continuous contact with water. Components used in hot-humidity environments, such as washing machine connectors or steam-exposed electrical housings, require end-use testing; published data for 1494X02 under sustained hot-water immersion are limited. If long-term hot-water resistance is required, a hydrolysis-stabilised PBT grade or another polymer may be necessary.
In terminal block bodies with brass inserts, the unfilled flame-retardant PBT grade is moulded around preheated inserts to reduce residual stress. Terminal insertion force testing after conditioning is part of the normal approval procedure because post-mould shrinkage can reduce hole size and increase insertion force. Local wall sections around inserts should be balanced to avoid premature freeze from the metal mass, and prototype measurements of hole diameter after 24 h ageing are used to determine the final pin-receiving tolerance.