| HS Code | 750836 |
| Polymer Type | PBT (polybutylene terephthalate) |
| Glass Fiber Content | 30% |
| Low Warp Characteristic | Yes |
| Density | 1.53 g/cm³ |
| Tensile Strength | 125 MPa |
| Elongation At Break | 2.5% |
| Flexural Strength | 190 MPa |
| Flexural Modulus | 8.5 GPa |
| Notched Charpy Impact Strength | 7 kJ/m² |
| Heat Deflection Temperature At 1 82 Mpa | 205 °C |
| Molding Shrinkage | 0.2–0.5% |
| Water Absorption | 0.07% |
| Flammability Rating | UL94 HB |
| Processing Method | Injection molding |
| Volume Resistivity | 1×10^16 Ω·cm |
As an accredited Toray Toraycon® PBT+GF30%-LW 7151G-X01 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Toray Toraycon® PBT+GF30%-LW 7151G-X01 is supplied in 25 kg moisture-proof bags, palletized for industrial storage and handling. |
| Container Loading (20′ FCL) | 20′ FCL: palletized 25 kg bags, typically up to 20 metric tons net, subject to carrier and destination weight limits. |
| Shipping | Toray Toraycon® PBT+GF30%-LW 7151G-X01 is shipped as non-hazardous, glass-fiber-reinforced polybutylene terephthalate pellets in sealed moisture-barrier bags or octabins. Keep dry and ventilated during transport, away from heat, humidity, UV, and contamination; avoid bag punctures. Protect packaging from physical damage, keep labels legible, and use standard freight conditions. No special dangerous-goods classification applies. |
| Storage | Store Toray Toraycon® PBT+GF30%-LW 7151G-X01 in a cool, dry, well-ventilated area away from direct sunlight, heat, flames, and moisture. Keep containers tightly closed and use original packaging to prevent contamination and dust ingress. Avoid prolonged humid exposure; dry before processing if supplier guidelines require. Follow local regulations and SDS recommendations. |
| Shelf Life | Shelf life is typically 12 months from manufacture when stored unopened in a cool, dry, well-ventilated area, away from moisture and sunlight. |
Competitive Toray Toraycon® PBT+GF30%-LW 7151G-X01 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Toraycon® PBT+GF30%-LW 7151G-X01 is a 30% glass-fibre-reinforced polybutylene terephthalate grade carrying a low-warpage modification. The grade is specified through ISO 1183-1 density, ISO 527-1/-2 tensile response, ISO 178 flexural modulus, ISO 179-1/1eA Charpy impact, ISO 75-1/-2 deflection temperature, and ISO 294-4 mould shrinkage. Its typical application envelope includes injection-moulded electrical and electronic housings, automotive sensor mounts, connector bodies, and structural appliance components where post-mould flatness and part-to-part positional tolerance are critical. The commercial designation “LW” indicates that the reinforcement package has been modified to reduce differential flow-direction versus transverse shrinkage relative to conventional 30% glass-fibre PBT; published filler composition data for 7151G-X01 is limited, but the effect is expressed through reduced warpage and improved dimensional predictability without eliminating the thermal resistance of the PBT matrix. For part designers, the grade is differentiated from unfilled PBT by higher flexural modulus and lower mould shrinkage, and from standard PBT GF30 by lower anisotropic distortion. It is generally processed as a pre-dried thermoplastic polyester; hydrolysis control is mandatory because melt-phase moisture above 0.02% by weight accelerates polymer chain scission. Exact lot-specific data should be obtained from the supplier’s certificate of analysis, because representative values in public datasheets are not specification limits.
The reinforcement architecture in 7151G-X01 consists of 30% by weight glass fibre dispersed in PBT; the low-warpage characteristic arises from a proprietary modification that minimises orientation-induced shrinkage anisotropy during solidification. In conventional GF30 PBT, flow-aligned fibres restrain shrinkage along the polymer orientation direction more than across it, producing a differential mould shrinkage that can exceed 0.4% between longitudinal and transverse directions. The LW modification reduces this differential, often to a range near 0.1% to 0.3% depending on part geometry, gate position, and wall thickness. This property is evaluated by ISO 294-4 using 60 mm × 60 mm × 2 mm plaques at melt and mould temperatures defined in the test procedure; product-specific shrinkage data for 7151G-X01 should be generated on the production tool because cavity pressure, fibre orientation, and cooling rate govern the final value. Density by ISO 1183-1 is typically in the 1.50–1.54 g/cm³ band for 30% GF PBT low-warp compounds; the presence of low-warpage additives may shift density relative to standard GF30 PBT. Ash content measured by ISO 3451-1 can be used to verify glass content, although a nominal 30% glass loading does not translate directly to 30% ash because the organic matrix and additives combust or degrade during the test. In mould-filling simulation, fibre orientation tensors for low-warpage grades must be calibrated against short-shot studies on the production tool; generic orientation parameters derived from standard GF30 PBT will overstate warpage in thin-walled parts.
Because standard 30% glass-fibre PBT grades show a useful balance of stiffness and heat resistance but suffer part distortion in flat, thin-walled parts, the comparative data below are used in material selection. The values are representative of commercial PBT families and are not lot-specific specifications for 7151G-X01.
| Property | Test method | 7151G-X01 representative | Standard PBT GF30 representative | Unfilled PBT representative |
|---|---|---|---|---|
| Density | ISO 1183-1 | 1.52 g/cm³ | 1.53 g/cm³ | 1.31 g/cm³ |
| Tensile strength at break | ISO 527-1/-2 | 125 MPa | 135 MPa | 55 MPa |
| Flexural modulus | ISO 178 | 9,000 MPa | 10,000 MPa | 2,600 MPa |
| Flexural strength | ISO 178 | 185 MPa | 200 MPa | 80 MPa |
| Charpy notched impact strength, 23 °C | ISO 179-1/1eA | 8.0 kJ/m² | 9.0 kJ/m² | 4.0 kJ/m² |
| Deflection temperature under load, 1.8 MPa | ISO 75-1/-2 | 200 °C | 205 °C | 55 °C |
| Mould shrinkage, flow/normal | ISO 294-4 | 0.2–0.5%/0.3–0.7% | 0.15–0.4%/0.6–1.0% | 1.6–2.0%/1.8–2.2% |
The distinction of 7151G-X01 is not a dramatic increase in tensile strength; it is the reduction in warpage while retaining most of the flexural modulus and heat resistance of standard GF30 PBT. Compared with mineral-filled low-warp PBT, the glass-reinforced LW grade retains higher notched impact strength and higher tensile strength. Compared with unfilled PBT, the 30% glass loading raises flexural modulus by a factor of roughly 3.5 and raises DTUL at 1.8 MPa from about 55 °C to about 200 °C. Elongation at break drops sharply; designers must avoid snap-fit designs that depend on base-resin ductility and should instead use flexible beam equations or finite-element models with the actual stress-strain curve from ISO 527-1/-2.
Pre-drying is mandatory for this grade because residual moisture reacts with the ester linkages in PBT at melt temperatures. A desiccant dryer set to 120 °C for 4–6 h, with a dew point below -30 °C, is used to reduce moisture to 0.02% or less. When ambient relative humidity exceeds 60%, the dried material should not remain exposed to plant air for more than 30 min; otherwise moisture regain occurs and hydrolysis resistance is reduced. Moisture measurement by ISO 15512 is appropriate for raw-material control. Melt-phase hydrolysis is the primary processing risk; therefore melt residence time at temperatures above 260 °C should be kept below 8 min. If the machine is interrupted, the barrel setpoint should be reduced by 20 °C and the screw purged with a low-viscosity PBT or polyester purge compound. Barrel temperature profiles normally run from 230–240 °C at the feed throat to 250–270 °C at the nozzle. The actual melt temperature, measured by an air shot, should not exceed 280 °C. At higher melt temperatures, fibre-matrix adhesion can decline and volatile degradation by-products can cause splay and surface deposits on the mould.
Mould surface temperature is a second process boundary. A range of 60–100 °C is commonly applied for reinforced PBT. Higher mould temperatures within this range improve crystallinity and reduce post-mould shrinkage and warpage, but increase cycle time. Mould temperatures below 60 °C can freeze orientation before crystallisation is complete, producing higher frozen-in stress and greater anisotropy. In flat parts, this conflict between dimensional stability and cycle time is resolved by running at 80–100 °C where geometric tolerance is critical, and by using conformal cooling channels if cycle-time constraints require higher heat extraction. Injection speeds should be moderate to fast; excessively high shear rates can fracture glass fibres and shift the fibre-length distribution toward shorter lengths, lowering tensile and impact properties. Back pressure in the range of 3–7 MPa hydraulic pressure is used to maintain melt homogeneity without excessive shear heating. Screw design should use a general-purpose metering screw with an L/D ratio of 18–22 and a compression ratio of 2.0–2.5:1; high-compression screws intended for polyolefins can generate unnecessary shear and fibre attrition. The non-return valve should be inspected for dead spots where PBT can stagnate and thermally degrade.
Hot-runner systems for 7151G-X01 require open-flow channel geometry with no stagnant regions, because PBT melt is sensitive to long thermal exposure. Valve-gate systems can be used, but gate temperature should be controlled independently and should not exceed the nozzle temperature. Cavity venting depth for glass-filled PBT is typically 0.02–0.03 mm; insufficient venting produces burn marks and irregular flow fronts. The low-warpage modification does not eliminate the need for correct gate placement. Single-edge gating of a flat rectangular housing will still produce an orientation bias; multiple gates or a film gate can reduce differential flow, but only if the melt fronts meet at angles that avoid high fibre orientation gradients. Weld lines in glass-reinforced PBT show lower strength than the bulk material; when weld lines are unavoidable, their position should be moved away from high-tensile regions, and the resulting strength reduction should be measured by ISO 527-1/-2 or ISO 178 on welded specimens.
For applications requiring flatness retention, dimensional stability is evaluated after moulding and after post-mould annealing at temperatures that simulate service exposure. Short-term shrinkage values are not sufficient for tolerance-stack analysis. Post-mould crystallisation of PBT can continue at service temperatures above 80 °C, producing small additional shrinkage. Annealing at 120 °C for 2–4 h can reduce subsequent dimensional drift, but part geometry should be checked for warpage after annealing because stress relaxation can release frozen-in orientation. Long-term creep data for this specific grade is limited; designers replacing metal with a low-warp PBT should request time-dependent modulus curves according to ISO 899-1 before committing to a structural design. Coefficient of linear thermal expansion measured by ISO 11359-2 for glass-reinforced PBT is generally in the range 2.5 × 10⁻⁵ K⁻¹ to 3.5 × 10⁻⁵ K⁻¹ below the glass transition; the low-warpage additives may shift directional expansion values, so product-specific data should be used for thermal tolerance calculations.
The primary comparison with PA66 occurs under humid service conditions. Glass-fibre-reinforced PA66 grades absorb moisture in the range of 5–6% at saturation when tested by ISO 62, while reinforced PBT grades generally absorb less than 0.5% water by weight. This difference means that PA66 dimensions and mechanical properties shift as moisture content changes, whereas PBT retains much closer to dry-as-moulded dimensions and stiffness. In electrical housings exposed to condensation or high humidity, the low-moisture absorption of PBT reduces tolerance stack-up and connector insertion-force variation. When PA66 is selected for high-temperature dry environments, its advantage diminishes; PBT GF30 offers similar DTUL at 1.8 MPa and better chemical resistance to many automotive fluids. Against die-cast aluminium or zinc, 7151G-X01 reduces mass because its density of about 1.52 g/cm³ is roughly 56% that of aluminium and 21% that of zinc. The substitution does not provide equivalent thermal conductivity or electromagnetic shielding; those functions must be supplied by design means such as metal inserts, shielding gaskets, or thermal pads.
Electrical properties should be confirmed per application. Dielectric strength is measured by IEC 60243-1, comparative tracking index by IEC 60112, and surface resistivity by IEC 62631-3-2. Product-specific published values for 7151G-X01 may be limited; the supplier should provide a complete electrical data package if the component is used in circuits above 60 V DC or in pollution degree 2 environments. Flammability classification under UL 94 must be confirmed on the final part thickness and colour, because thin-wall sections and certain pigments can change the classification. For applications requiring a V-0 listing, a separate flame-retardant PBT grade should be evaluated rather than assuming that glass reinforcement alone provides flame retardance.
Processing and service boundaries include avoiding prolonged contact with hot water above 80 °C, strong acids, or strong alkaline environments, unless validated by ISO 175 immersion testing. Where a part is exposed to hot oil, brake fluid, or diesel, chemical compatibility should be tested at the maximum service temperature and for the expected contact duration, because PBT can crystallise further and become embrittled under aggressive chemical load. The low-warpage modification does not override the fundamental hydrolysis sensitivity of PBT in hot aqueous environments. Regrind use should be controlled; glass-fibre length decreases with each regrind cycle, and adding more than 25% regrind is generally not advisable without mechanical testing of the moulded components. The grade should be kept separate from acetal and polyamide regrind streams, because cross-contamination can cause delamination, gas evolution, or incompatible crystallisation behaviour.