| HS Code | 417243 |
| Glassfibercontent | 30% |
| Density | 1.53 g/cm³ |
| Tensilestrength | 140 MPa |
| Elongationatbreak | 2.5% |
| Flexuralmodulus | 9,300 MPa |
| Flexuralstrength | 210 MPa |
| Charpynotchedimpactstrength | 8 kJ/m² |
| Hdt 1 82mpa | 205 °C |
| Meltingpoint | 225 °C |
| Waterabsorption 24h | 0.07% |
| Moldingshrinkage Flow | 0.2–0.5% |
| Moldingshrinkage Crossflow | 0.5–0.9% |
| Volumeresistivity | 1×10^16 Ω·cm |
| Dielectricconstant 1mhz | 3.5 |
| Dielectricstrength | 20 kV/mm |
| Arcresistance | 120 s |
As an accredited Toray Toraycon® PBT+GF30% 1101G-30 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 25 kg moisture-barrier bags, Toray Toraycon® PBT+GF30% 1101G-30 is typically palletized for industrial handling. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with Toray Toraycon® PBT+GF30% 1101G-30 in original sealed packaging, palletized and secured for export shipment. |
| Shipping | Toray Toraycon® PBT+GF30% 1101G-30 is generally shipped as non-hazardous, moisture-sensitive plastic resin pellets in sealed bags or containers. No UN number or hazard class is normally assigned. Protect from heat, humidity, and contamination; follow the SDS and local transport regulations. |
| Storage | Store Toray Toraycon® PBT+GF30% 1101G-30 in a cool, dry, well-ventilated area, protected from direct sunlight, heat, moisture, and strong oxidizers. Keep original containers sealed until use and avoid excessive stacking or damage. Maintain stable, moderate temperatures and low humidity; follow the supplier’s SDS and local regulations. Do not store near ignition sources or incompatible materials. Use first-in, first-out stock rotation. |
| Shelf Life | Typically two years from manufacture when stored dry, cool, and in sealed original packaging; protect from moisture. |
Competitive Toray Toraycon® PBT+GF30% 1101G-30 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Toray Toraycon® PBT+GF30% 1101G-30 is an injection-moulding compound of polybutylene terephthalate containing 30% by weight short-glass fibre. Under ISO 1043-1:2011 the designation is PBT-GF30; under ISO 7792-1:2012 it is classified within the thermoplastic polyester moulding and extrusion material group. The product is supplied in pellet form and is intended for melt processing at 245°C to 265°C. Its primary distinction from unfilled PBT grades is higher tensile modulus, higher flexural modulus, lower mould shrinkage, and greater load-bearing capacity at elevated temperature; its primary limitation is low tensile elongation at break and corresponding sensitivity to sharp notches.
The compound is normally moulded on conventional reciprocating-screw injection moulding machines. Because glass fibre increases melt viscosity and abrasive wear, plasticising units with bimetallic or hardened barrels and screws are specified for extended runs. The feedstock is hygroscopic only to a limited extent, but the ester backbone of PBT is hydrolytically sensitive at melt temperature, so drying below 0.02% residual moisture is more critical than preventing splay alone.
Representative values obtained from standard test specimens are listed below. These are typical lot-average values, not minimum specification limits, and they are obtained only when the material is dried and moulded under controlled conditions.
| Measured property | Test method | Typical value |
|---|---|---|
| Density | ISO 1183-1:2019 | 1.53 g/cm³ |
| Tensile stress at break | ISO 527-1/-2:2012 | 135 MPa |
| Tensile strain at break | ISO 527-1/-2:2012 | 2.5 % |
| Flexural strength at break | ISO 178:2019 | 200 MPa |
| Flexural modulus | ISO 178:2019 | 9,500 MPa |
| Charpy notched impact, 23°C | ISO 179-1/1eA:2010 | 9 kJ/m² |
| Charpy unnotched impact, 23°C | ISO 179-1/1eU:2010 | 40 kJ/m² |
| Heat deflection temperature, 1.8 MPa | ISO 75-1/-2:2013 | 205 °C |
| Heat deflection temperature, 0.45 MPa | ISO 75-1/-2:2013 | 220 °C |
| Mould shrinkage, flow direction | ISO 294-4:2018 | 0.2–0.4 % |
| Mould shrinkage, transverse direction | ISO 294-4:2018 | 0.7–1.0 % |
| Water absorption, 24 h at 23°C | ISO 62:2008 | 0.07 % |
The tensile stress at break of 135 MPa and flexural modulus of 9,500 MPa are achieved after proper drying and with test bars moulded under conditions that orient fibres in the flow direction. Cross-flow or weldline properties are lower because glass fibres do not bridge the weld plane; welded tensile strength can fall to 50–60% of unwelded tensile strength depending on gate configuration. Elongation at break of 2.5% means that snap-fit arms require generous radii and low strain. The material is not an impact-modified compound and should not be treated as a ductile resin. Charpy notched impact of 9 kJ/m² confirms sensitivity to sharp corners; the unnotched value of 40 kJ/m² shows substantially better energy absorption when corner radii are increased above 0.5 mm.
Before melt processing, pellets are dried at 120°C for 4 h or 130°C for 3 h in a desiccant dryer with a dew point of -30°C or lower. Hot-air drying is not sufficient when ambient relative humidity exceeds 60% because the polyester matrix can exceed the target moisture level. Residual moisture above 0.02% causes hydrolysis during plastication; the first indications are reduced melt viscosity and surface streaking, but tensile strength and impact values may drop even on visually acceptable parts. Regrind should be dried separately for a longer time and held below 20% by weight in non-safety applications. Each screw cycle reduces glass fibre length, so higher regrind ratios reduce notched Charpy impact disproportionately.
In production on a 1200 kN hydraulic injection moulding machine with a 40 mm bimetallic three-zone screw, the rear zone is normally set at 240–245°C, the centre zone at 250–255°C, the front zone at 260–265°C, and the nozzle at 255–265°C. Mould-wall temperature is controlled at 70–90°C for structural parts requiring flatness; lower mould temperatures of 40–60°C shorten cycle time but increase frozen-layer orientation and anisotropic warpage. Injection velocity should be moderate to high, and shot volume should be between 40% and 70% of barrel capacity to limit residence time. A screw decompression of 2–5 mm after recovery prevents nozzle drool, but excessive suck-back can draw air into the melt and oxidise the PBT.
Rheologically, 1101G-30 shows shear-thinning behaviour typical of glass-filled PBT. Melt volume-flow rate under ISO 1133-1:2022 at 250°C and 2.16 kg is generally reported in the range 10–20 cm³/10 min, but the value is sensitive to residual moisture and capillary flow orientation. The fibre phase raises viscosity at low shear rates, producing a more pronounced shear-thinning response than unfilled PBT. In thin-walled mouldings this leads to high shear at the frozen skin and explicit fibre alignment parallel to flow, while the core may retain more random orientation. Weldlines form as fibre-free interfaces between opposing flow fronts; their location should be mapped by short-shot trials before production tooling is finalised.
Hot-runner systems for this grade require fully heated nozzles and manifold temperatures no higher than 270°C. Dead spots in open nozzles or poorly swept runner drops can lead to black specks after extended residence. Standard cold-runner sprue and runner diameters should be larger than those used for unfilled PBT by approximately 0.5–1.0 mm to compensate for increased melt stiffness at low shear rates.
At 1.8 MPa, the heat deflection temperature of 205°C places 1101G-30 above unfilled PBT, whose DTUL is typically 140–150°C under the same load. The 0.45 MPa value of 220°C is relevant for low-stress electrical housings exposed to wave soldering or vapour-phase reflow. Continuous use in air above 130°C should nevertheless be validated by oven ageing; the heat stabiliser package retards oxidative embrittlement but does not eliminate long-term surface cracking.
Dimensional stability is anisotropic. Fibre orientation reduces in-flow shrinkage to 0.2–0.4% and leaves transverse shrinkage at 0.7–1.0%. Parts with a single edge gate tend to bow toward the low-shrinkage direction after demoulding. Multiple edge gates, a film gate, or a centrally placed diaphragm gate reduce this asymmetry. The coefficient of linear thermal expansion under ISO 11359-2 is typically lower in the flow direction and higher across flow; differences of roughly 2–3×10⁻⁵ K⁻¹ in flow and 6–8×10⁻⁵ K⁻¹ transverse have been reported for glass-filled PBT grades, but moulded-part gating must be considered because the test plaque is not isotropic.
In volume electrical and electronic component production, 1101G-30 is used for board-mounted relay housings, coil bobbins, circuit-breaker internal frames, power-tool housings, automotive connector bodies, sensor housings, and ignition-coil cases. These applications exploit the combination of high flexural modulus, low creep under clamp load, and low water absorption. In 2.54 mm pitch pin headers, the low in-flow mould shrinkage permits pin-to-pin position tolerances below ±0.05 mm after conditioning at 23°C and 50% relative humidity. Weldlines should not pass through pin rows; if unavoidable, the gate should be relocated via short-shot trials to move the weldline to a low-stress region.
Replacement of POM or PA66 is usually driven by the need for better dimensional retention in moisture or by lower moisture-induced electrical property drift. At equilibrium with 23°C and 50% relative humidity, PBT/GF30 absorbs roughly 0.07% water, while PA66 can absorb 1.5–2.5%. The lower water uptake stabilises volume resistivity and surface leakage behaviour through the connector wall. Compared with POM, PBT/GF30 has a higher heat deflection temperature under 1.8 MPa but lower notched impact and lower elongation. POM can offer better snap-fit deflection in dry conditions, while PBT/GF30 provides better dimensional stability in warm-humid electrical environments. A direct drop-in substitution is not automatic because the glass-filled polyester has higher melt viscosity and lower ductility than many acetal grades.
Electrical properties of glass-filled PBT are structure-sensitive. Dry moulded volume resistivity is usually of the order of 10^14–10^15 Ω·cm under IEC 62631-3-1:2016, and short-time dielectric strength under IEC 60243-1:2013 is typically 20–25 kV/mm at 1.0 mm thickness. Glass fibres lower the comparative tracking index relative to unfilled PBT because exposed fibre ends and fibre-matrix interfaces create local field concentrations and tracking paths. The grade is not recommended for primary insulation where creepage and clearance distances are already at the regulatory minimum; end-product testing to IEC 60664-1 or the applicable product standard is required. The standard natural grade is typically classified under UL 94 HB. Electrical enclosures requiring V-0, V-1, or glow-wire ignition resistance at 750°C or 850°C require flame-retardant Toraycon grades or a halogen-free flame-retardant PBT/GF30, not 1101G-30.
The PBT matrix contains ester linkages that undergo hydrolysis in the presence of water at elevated temperature. The grade is stable in normal indoor humidity and occasional condensation, but continuous immersion in water above 60°C or exposure to steam is not recommended. Hydrolysis is temperature-dependent and begins at the moulded surface, producing molecular-weight loss and embrittlement even when bulk stiffness appears acceptable. Hot aqueous alkaline solutions at pH 10 or above and hot aqueous ethylene glycol/water mixtures used in engine coolant are specific incompatibility boundaries. Validation should include mechanical property retention after fluid immersion, not visual inspection alone.
Contact with primary or secondary amines at processing temperature should be excluded because amine attack accelerates chain scission through aminolysis and can reduce melt viscosity and impact strength even when the amine is present as a low-level external lubricant or release-agent residue. Silicone-based mould releases and hydrocarbon waxes are generally lower risk. Resistance to aromatic and aliphatic hydrocarbons, alcohols, and chlorinated solvents is moderate to good at room temperature, but strong acids and phenols attack the polyester. Regrind sourced from parts that have contacted aggressive fluids should be validated separately before reuse.