| HS Code | 949606 |
| Polymer Type | PBT (polybutylene terephthalate) |
| Glass Fiber Content | 15% |
| Density | 1.41 g/cm³ |
| Tensile Strength | 98 MPa |
| Tensile Elongation At Break | 3.0% |
| Flexural Modulus | 5,390 MPa |
| Flexural Strength | 147 MPa |
| Notched Izod Impact Strength 23c | 5.9 kJ/m² |
| Hdt 1 82mpa | 199°C |
| Melting Point | 224°C |
| Water Absorption 24h | 0.07% |
| Mold Shrinkage Flow | 0.4–0.6% |
| Mold Shrinkage Cross Flow | 1.0–1.4% |
| Ul94 Flame Rating | HB |
| Volume Resistivity | 1×10^16 Ω·cm |
| Dielectric Strength | 20 kV/mm |
As an accredited Toray Toraycon® PBT+GF15% 1201G-15 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Toray Toraycon® PBT+GF15% 1201G-15 is packed in 25 kg moisture-barrier bags, palletized and shrink-wrapped for shipment. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): palletized, shrink-wrapped bags of Toray Toraycon® PBT+GF15% 1201G-15 secured inside a 20′ FCL for ocean freight. |
| Shipping | Toray Toraycon® PBT+GF15% 1201G-15 is shipped as dry, glass-fiber-reinforced PBT pellets in sealed moisture-barrier bags, boxes, or octabins. Keep containers closed and store in a dry, ventilated area away from heat and direct sunlight; typically no dangerous-goods classification applies. |
| Storage | Store Toray Toraycon® PBT+GF15% 1201G-15 in a cool, dry, well-ventilated area away from direct sunlight, heat sources, and moisture. Keep material in original sealed packaging until use to prevent contamination and moisture pickup. Avoid prolonged humid exposure; if damp, dry according to supplier recommendations before processing. Observe local safety and housekeeping regulations. |
| Shelf Life | Toray Toraycon® PBT+GF15% 1201G-15 has a shelf life of about two years when kept in original sealed packaging, dry and cool. |
Competitive Toray Toraycon® PBT+GF15% 1201G-15 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Toray Toraycon® PBT+GF15% 1201G-15 is a short-glass-fibre-reinforced polybutylene terephthalate injection-moulding grade containing 15 wt% glass fibre by mass. The filler loading places the material between unfilled PBT and 30 wt% glass-reinforced PBT in the 1201G series. Typical published datasheet values place density at 1.41–1.43 g/cm³ under ISO 1183-1, melt flow rate in the range of 18–26 g/10 min at 250 °C with 2.16 kg load under ISO 1133-1:2022, and melting endotherm near 223–225 °C by differential scanning calorimetry under ISO 11357-3. The 15 wt% glass loading corresponds to roughly 7–9 vol% fibre at this density range. The base resin retains the semi-crystalline polyester structure of PBT, giving a sharp solidification response that can shorten cycle time but also creates crystallinity gradients across section thickness when mould temperature is too low.
The designation 1201G-15 identifies the general-purpose glass-reinforced grade family and the nominal filler weight fraction. Unlike unfilled 1201G grades, the reinforcement modifies tensile modulus, notched impact response, heat deflection temperature and mould shrinkage. The final mechanical response after injection moulding is governed substantially by residual fibre length retained through screw recovery, plastication and gate flow, not by the original pellet length.
The primary processing boundary is residual moisture. PBT is an ester-linked thermoplastic, and water above the producer limit initiates hydrolysis of the terephthalate ester bonds during plasticating. Desiccant drying at 120 °C for 4–8 h to a final moisture content below 0.02% is specified for the 1201G series. On production-scale machines of 80–120 tonnes clamp force, non-dried pellets or material exposed to ambient air above 60% RH for more than 30–60 min after drying can produce silver streaks, erratic nozzle pressure, gate blush and measurable loss of notched Charpy impact strength under ISO 179-1/1eA. The failure mode observed on hydraulic toggle presses is often a sudden decrease in melt viscosity due to polymer chain scission, followed by short shots and delamination at weld lines. Hopper dryers used in continuous moulding should maintain the feed throat with a dry-air dew point of ≤ −30 °C. Desiccant dryer airflow of 30–60 L/min per 100 kg/h throughput is a practical production guideline.
Glass-fibre attrition during screw recovery is a second process conflict. Screw speed above 0.25 m/s peripheral velocity or back pressure above 5 MPa increases breakage of short glass fibres, reducing residual fibre length and tensile strength under ISO 527-2. General-purpose screws with 18:1–22:1 L/D, compression ratio of 2.5:1–3.0:1 and a free-flow non-return valve are used. High-compression mixing screws are not required and can overheat the melt. Barrel residence time should be kept below 5 min, and melt temperature should not exceed 270 °C except during brief interruptions. At longer residence or high temperature, thermal oxidation discolours the part and deposits degraded PBT on the screw root, producing black specks.
During injection moulding of thin-wall connectors, a nozzle melt temperature of 250–260 °C is commonly used, with rear-zone barrel setpoints near 230–240 °C and front-zone setpoints near 255–265 °C. Mould temperature is controlled at 40–80 °C; the lower range shortens cooling time but may freeze a low-crystallinity skin, while the upper range improves dimensional stability but extends cycle time. Transfer pressure is typically in the 80–100 MPa hydraulic range for wall thicknesses of 1.0–2.0 mm, and holding pressure of 60–80 MPa for 3–6 s is used to compensate solidification shrinkage. Fill time should be fast enough to prevent premature freeze-off at the gate: 0.5–1.5 s for multi-pin connectors with gate diameters of 0.8–1.2 mm. Clamp force requirements are approximately 0.5–0.8 tonnes/cm² projected area for glass-filled PBT, although thick bosses and long flow lengths shift the requirement upward.
| Property | Test standard | 1201G-15 typical range | Unfilled PBT typical range | 30% glass-filled PBT typical range |
|---|---|---|---|---|
| Density | ISO 1183-1 | 1.41–1.43 g/cm³ | 1.30–1.32 g/cm³ | 1.50–1.54 g/cm³ |
| Tensile strength at break | ISO 527-2 | 100–115 MPa | 50–60 MPa | 130–150 MPa |
| Tensile modulus | ISO 527-2 | 5,000–5,600 MPa | 2,400–2,700 MPa | 8,500–10,000 MPa |
| Flexural modulus | ISO 178 | 4,800–5,500 MPa | 2,200–2,600 MPa | 8,000–9,500 MPa |
| Notched Charpy impact at 23 °C | ISO 179-1/1eA | 5.0–6.1 kJ/m² | 3.0–4.4 kJ/m² | 7.0–9.5 kJ/m² |
| Heat deflection temperature at 1.80 MPa | ISO 75-2 | 185–205 °C | 50–60 °C | 200–215 °C |
| Mould shrinkage, flow direction | ISO 294-4 | 0.6–0.8% | 1.5–2.0% | 0.3–0.6% |
The comparison shows that 15 wt% fibre raises flexural modulus by roughly a factor of two relative to unfilled PBT, whereas a 30 wt% glass grade raises it by three to four times. The elongation at break of 1201G-15 falls to approximately 3.0–4.0% under ISO 527-2, removing the ductile yielding characteristic of unfilled PBT. However, the lower filler fraction produces less anisotropic shrinkage than a 30 wt% compound in flat multi-gate housings. When dimensional stability is the primary concern, 1201G-15 is evaluated against unfilled PBT for warpage, sink marks and post-mould shrinkage using ISO 294-4 after 48 h at 23 °C and 50% RH.
In automotive relay bases, sensor connectors and under-hood housings, the grade is used for low- to medium-voltage insulating parts. Relevant electrical values include volume resistivity above 10¹⁴ Ω·cm under IEC 62631-3-1 and dielectric strength commonly reported in the 20–25 kV/mm range for 3.0 mm specimens under IEC 60243-1. Comparative tracking index is frequently listed between 200 V and 250 V under IEC 60112. Flammability is normally UL 94 HB; if a V-0 classification is required, flame-retardant PBT grades are used instead. Published data for continuous-use temperature ratings in specific colours and thicknesses may be limited; end-use thermal ageing validation under ISO 2578 is required before substitution into safety-related components.
Where 1201G-15 is compared with 30% glass-filled PBT, the lower glass content is decisive for flatness, gate-area stress and tool wear. The 15 wt% filler fraction reduces density and abrasive wear on steel tooling, screw flights and gate inserts relative to a 30 wt% short-glass compound, but it cannot match the modulus of the higher-fibre grade. Compared with unfilled PBT, 1201G-15 reduces mould shrinkage and provides higher stiffness, but loses impact strength and surface smoothness. This positions the grade for moderate load-bearing parts where dimensional stability is more important than maximum rigidity.
When prolonged contact with hot water above 70 °C or alkaline cleaning baths is specified, 1201G-15 should be evaluated with hydrolysis testing under ISO 62 and tensile testing under ISO 527-2; glass-reinforced PBT can still undergo chain scission at the fibre-matrix interface. The material should not be processed in systems contaminated with polyamide or PVC because residual acid or amine species can catalyse ester degradation. If hot-runner downtime exceeds 10 min, the manifold and drool bushing should be purged or dropped to standby temperature below 180 °C to prevent thermal degradation and gate clogging. Polyamide purges are avoided for glass-filled PBT; a compatible general-purpose purge compound or HDPE-based purge is preferred before shutting down the barrel.