| HS Code | 708838 |
| Density | 1.36 g/cm³ |
| Melting Point | 265 °C |
| Glass Transition Temperature | 120 °C |
| Intrinsic Viscosity | 0.65 dL/g |
| Water Absorption | 0.30 % |
| Tensile Strength | 80 MPa |
| Tensile Modulus | 3.0 GPa |
| Elongation At Break | 3.0 % |
| Flexural Modulus | 3.2 GPa |
| Heat Deflection Temperature At 1 82 Mpa | 100 °C |
| Coefficient Of Linear Thermal Expansion | 20 ppm/°C |
| Dielectric Constant At 1 Mhz | 3.0 |
| Dissipation Factor At 1 Mhz | 0.002 |
| Volume Resistivity | 1.0E+16 Ω·cm |
| Ul Flammability Rating | HB |
As an accredited Teijin Limited Teonex® PEN Resin TN-8065S factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg moisture-resistant bags on pallets, clearly labeled Teonex® PEN Resin TN-8065S with lot and handling information. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with Teijin Limited Teonex® PEN Resin TN-8065S in sealed packaging, palletized and secured for ocean shipment. |
| Shipping | Teonex® PEN Resin TN-8065S is shipped as a non-hazardous solid polymer resin. It is not classified as dangerous goods for transport under DOT, IMDG, IATA, or ADR; no UN number, proper shipping name, hazard class, or packing group applies. Use standard industrial packaging and follow local regulations. |
| Storage | Store Teonex® PEN Resin TN-8065S in a cool, dry, well-ventilated area away from direct sunlight, heat, ignition sources, and incompatible materials. Keep containers tightly closed to prevent moisture pickup and contamination. Use original packaging, avoid prolonged high-temperature exposure, and follow the manufacturer’s SDS and local regulations for specific shelf-life and handling requirements. |
| Shelf Life | Typically 12 months from manufacture when stored unopened in original packaging, dry, cool, and protected from moisture and sunlight. |
Competitive Teijin Limited Teonex® PEN Resin TN-8065S prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Teijin Limited supplies Teonex® PEN Resin TN-8065S as a polyethylene naphthalate homopolymer for extrusion and injection moulding. The polymer chain contains naphthalene-2,6-dicarboxylate units, which replace the benzene-1,4-dicarboxylate units of conventional polyethylene terephthalate. The rigid fused aromatic ring increases the glass transition temperature to approximately 121 °C and the crystalline melting point to approximately 265 °C. Unfilled moulded density is typically 1.33–1.36 g/cm³ when measured according to ISO 1183-1:2019. The product is supplied as pellets and is specified for applications requiring higher thermal performance and lower oxygen permeation than PET. It is not a drop-in replacement for PET. Barrel temperatures, mould temperatures and drying conditions must be adjusted. Published data for this specific configuration is limited for TN-8065S; the supplier’s certificate of analysis should be used for critical design values.
The grade differs from PET and PBT in three measurable properties: thermal resistance, barrier behaviour, and ultraviolet absorption. The glass transition of TN-8065S is approximately 43 °C higher than that of PET and approximately 76 °C higher than that of PBT. The melting point is approximately 15 °C higher than PET and approximately 42 °C higher than PBT. These differences permit short-term exposure to temperatures that would soften PET parts and reduce dimensional stability in PBT components. The naphthalate structure also reduces oxygen permeability in oriented films to roughly one-third to one-fifth of PET at 23 °C and 0 % RH, as reported in polymer barrier literature under ASTM D3985-17. These advantages are balanced by higher raw-material cost, more aggressive drying requirements and a narrower thermal processing window.
In differential scanning calorimetry under ISO 11357-2:2020, PEN homopolymer exhibits a glass transition near 121 °C and a melting endotherm near 265 °C. PET typically shows a glass transition near 78 °C and a melting point near 250 °C. The difference in glass transition is not simply a linear function of backbone stiffness; it reflects reduced free volume and restricted segmental motion caused by the fused aromatic naphthalene unit. In practical terms, biaxially oriented films retain measurable mechanical properties at temperatures 20–30 °C above comparable PET films, although oxidative stability is still controlled by the antioxidant package and end-use environment.
Oxygen permeability coefficients reported for biaxially oriented PEN films range from 1.0 cm³·mm/m²·day·atm to 1.5 cm³·mm/m²·day·atm at 23 °C and 0 % RH. PET films of equal thickness are commonly cited at 2.5–3.5 cm³·mm/m²·day·atm under the same conditions. The barrier improvement is attributed to reduced segmental mobility and lower gas diffusion rather than solubility differences. This property supports use in packages where oxidative degradation or flavour loss is critical.
The crystallization half-time of PEN is longer than PET at equivalent undercooling. Isothermal DSC measurements indicate that PEN crystallizes slowly; optical haze in thick-wall parts is therefore controlled by mould temperature rather than by nucleating agents alone. The slower crystallization widens the window for transparent injection moulding only if the mould is run hot. At mould temperatures below 120 °C, quenched amorphous material remains dimensionally unstable and may densify during later thermal exposure.
| Property | TN-8065S PEN | PET reference | PBT reference | Standard |
|---|---|---|---|---|
| Glass transition temperature | 121 °C | 78 °C | 45 °C | ISO 11357-2:2020 |
| Crystalline melting point | 265 °C | 250 °C | 223 °C | ISO 11357-3:2018 |
| Specific gravity | 1.36 | 1.34 | 1.31 | ISO 1183-1:2019 |
| Tensile strength at break | 75 MPa | 55 MPa | 50 MPa | ASTM D638-14 |
| Tensile modulus | 2.4 GPa | 2.1 GPa | 2.5 GPa | ASTM D638-14 |
| Oxygen permeability coefficient, biaxially oriented film | 1.2 cm³·mm/m²·day·atm | 3.0 cm³·mm/m²·day·atm | Not commonly reported | ASTM D3985-17 |
Values are unfilled polymer literature data for screening comparisons, not specification limits for TN-8065S. Lot-specific data should be obtained from Teijin technical documentation.
Drying before melt processing is mandatory for TN-8065S. At plant relative humidity above 60 %, pellets absorb moisture rapidly; hydrolysis reduces intrinsic viscosity and creates surface defects in extruded film and injection moulded parts. Desiccant drying at 160–170 °C for 4–6 h with a dew point of −30 °C or lower is recommended. Residual moisture must be held below 0.005 % (50 ppm). Closed-loop conveying and hopper dryers are preferred. In moisture-sensitive production, a return-air dew-point monitor should alarm at −20 °C.
Extrusion processing of TN-8065S uses barrel profiles from 280 °C at the feed throat to 310 °C at the metering zone. Melt temperature measured by immersion pyrometer should remain at 300 °C ±5 °C. Single-screw extruders with L/D of 30:1 to 36:1 and twin-screw extruders with L/D of 32:1 to 40:1 are suitable. Screw speed should be limited to 50–100 min⁻¹ for 40 mm diameter single-screw machines to avoid excessive shear heating. Vacuum venting at −0.08 MPa gauge is applied after plastication. Extended residence time above 10 min at melt temperatures above 300 °C increases crystalline reorganisation and gel formation.
Injection moulding with TN-8065S requires mould temperatures between 120 °C and 150 °C. Cavity surface temperature should be confirmed by contact pyrometry instead of machine setpoint. A cavity-surface distribution outside a ±5 °C tolerance across a multi-cavity tool generates differential crystallinity, anisotropic shrinkage and warpage in flat parts. On machines with 1,200–2,500 kN clamp force, injection pressure is typically 80–120 MPa; hold pressure is 40–60 MPa; back pressure is 0.5–1.5 MPa. Screw rotation of 50–100 min⁻¹ is adequate. Nozzle temperature should be 295–305 °C. Moulds below 100 °C produce amorphous skins that densify during later thermal exposure and cause post-mould dimensional movement.
Hot-runner systems for TN-8065S operate at manifold temperatures of 290–305 °C and nozzle-tip temperatures of 300 °C. Gate orifices smaller than 1.5 mm elevate shear heating and may generate silver streaks and gate blush. Valve-gate actuation should complete within 0.5 s to avoid premature freeze-off at the gate. Dead-flow zones longer than 10 mm without purge cause stagnation, leading to black specks and viscosity drift. Production trials on technical parts have traced black specks to hot-runner drops with insufficient thermal uniformity, not to the base resin. Hot-runner controllers should hold each nozzle zone within ±2 °C of setpoint. If a valve-gate system is not purged during colour change, carbonaceous residue can detach into the next shot.
Incompatibilities include amine-based additives, which attack ester linkages through aminolysis and reduce molecular weight. Acidic flame-retardant masterbatches and chlorinated polymers in re-grind should be excluded because acid evolution accelerates hydrolysis at processing temperatures. Regrind content should not exceed 20 wt% unless viscosity retention is confirmed by intrinsic viscosity measurement. Blending with PET alters crystallization kinetics and should not be performed without pilot-scale evaluation.
In biaxially oriented film production, TN-8065S is typically cast at 285–295 °C, then machine-direction stretching is performed at 145–155 °C and transverse-direction stretching at 150–160 °C. Heat-setting at 230–240 °C for 10–20 s stabilises the oriented film. Oriented PEN film shows higher modulus and lower shrinkage than PET at equivalent draw ratios. Applications include flexible printed circuit substrates, high-temperature capacitor films, thermal transfer ribbons, and dimensional-stable labels. In these applications, property requirements are typically specified by IPC-TM-650 test methods or by internal electrical standards. Published data for this specific configuration is limited for TN-8065S because film property values depend on draw ratio, heat-setting temperature and line speed.
The resin is also used in melt-spun fibres where tenacity and modulus retention at elevated temperature are required. In fibre spinning, take-up speeds and draw ratios are adjusted to compensate for the slower stress-induced crystallization of PEN compared with PET. Industrial use of TN-8065S has also been reported in release liners, high-temperature labels and injection-moulded sensor housings. Each application requires separate verification of mechanical, electrical and thermal properties according to ASTM D638-14, ASTM D648-18, ASTM D149-20, and UL 746B where applicable.
Regulatory compliance for TN-8065S is end-use dependent. Food-contact status should be evaluated by the finished-article manufacturer. Polyethylene naphthalate polymers are referenced in 21 CFR 177.1632; migration testing under 21 CFR 177.1630 conditions may be needed if the article is used in contact with food. European food-contact use must comply with EU 10/2011 and its amendments; overall migration and specific migration limits are determined on the finished article, not the resin alone. Electrical and electronic applications should be assessed under RoHS Directive 2011/65/EU Annex II and REACH Article 33 SVHC communication obligations. Standard UL Yellow Card ratings are grade-specific and must be confirmed through the UL iQ database for TN-8065S.
| Framework | Applicability to TN-8065S | Verification requirement |
|---|---|---|
| FDA 21 CFR 177.1632 | Polyethylene naphthalate polymers for food-contact articles | Finished-article extraction and migration testing |
| EU 10/2011 | Plastic food-contact materials | Overall migration and specific migration limit evaluation |
| RoHS 2011/65/EU | Electrical and electronic equipment components | XRF screening and confirmatory chemical analysis |
| REACH Article 33 | SVHC content above 0.1 wt% | Supplier SVHC confirmation |
Substitution of PET or PBT with TN-8065S is not a direct material swap. The higher melt temperature requires barrel and hot-runner changes; the higher mould temperature increases cooling time and energy demand. Components with wall thickness above 4 mm may exhibit sink marks and crystallinity variation. Chemical resistance in alkaline and strongly acidic environments should be tested because the polyester backbone hydrolyzes under extreme pH. For outdoor exposure, UV stability is improved relative to PET but long-term weathering still requires stabilisation or coating. Parts should be annealed or moulded with hot tooling if dimensional tolerances below 0.1 % over a −40 °C to 150 °C service range are specified.