Sinopec Zhongke Hdpe 5000s 5502

Sinopec Zhongke HDPE 5000S / 5502

    • Product Name: Sinopec Zhongke HDPE 5000S / 5502
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 211552
    Manufacturer Sinopec Zhongke
    Product Name Sinopec Zhongke HDPE 5000S / 5502
    Polymer Type High Density Polyethylene (HDPE)
    Grade 5000s Density 0.954 g/cm3
    Grade 5000s Melt Flow Rate 0.9 g/10min
    Grade 5000s Tensile Yield Strength >=24 MPa
    Grade 5000s Elongation At Break >=500 %
    Grade 5000s Flexural Modulus >=900 MPa
    Grade 5000s Vicat Softening Point >=125 °C
    Grade 5000s Brittleness Temperature <=-70 °C
    Grade 5000s Notched Izod Impact Strength >=15 kJ/m2
    Grade 5000s Shore D Hardness 60
    Grade 5000s Melting Point 130-135 °C
    Grade 5000s Processing Method Extrusion
    Grade 5000s Typical Applications Monofilament, rope, net, packaging tape
    Grade 5502 Density 0.955 g/cm3
    Grade 5502 Melt Flow Rate 0.2 g/10min
    Grade 5502 Tensile Yield Strength >=26 MPa
    Grade 5502 Elongation At Break >=600 %
    Grade 5502 Flexural Modulus >=1000 MPa
    Grade 5502 Vicat Softening Point >=126 °C
    Grade 5502 Brittleness Temperature <=-70 °C
    Grade 5502 Notched Izod Impact Strength >=20 kJ/m2
    Grade 5502 Shore D Hardness 62
    Grade 5502 Melting Point 130-135 °C
    Grade 5502 Processing Method Blow Molding, Extrusion
    Grade 5502 Typical Applications Blow molded containers, bottles, industrial parts

    As an accredited Sinopec Zhongke HDPE 5000S / 5502 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Sinopec Zhongke HDPE 5000S/5502 is packaged in 25 kg PP woven bags or 1000 kg jumbo bags; bulk available.
    Container Loading (20′ FCL) 20′ FCL container loading of Sinopec Zhongke HDPE 5000S/5502, 25kg bags, palletized or loose, securely stowed for safe ocean transport.
    Shipping Sinopec Zhongke HDPE 5000S/5502 is shipped as non-hazardous polyethylene pellets in 25 kg woven bags, palletized and stretch-wrapped. Standard 20-foot containers hold about 25 MT. Transport and store in dry, ventilated conditions, away from direct sunlight, moisture, heat, and contamination. Handle with normal industrial hygiene.
    Storage Store Sinopec Zhongke HDPE 5000S/5502 in a cool, dry, well-ventilated warehouse, away from direct sunlight, rain, moisture, heat, flames, and strong oxidizers. Keep original packaging sealed and stack securely to prevent damage. Avoid contamination with dust, dirt, or other polymers. Maintain clean, ambient conditions; no special refrigeration required. Observe local fire and material-handling regulations.
    Shelf Life Typically 24 months when stored unopened in a cool, dry, well-ventilated area, away from direct sunlight and heat.
    Application of Sinopec Zhongke HDPE 5000S / 5502

    In extrusion blow moulding of small- and medium-volume rigid packaging, Sinopec Zhongke HDPE 5502 is processed on continuous shuttle machines and intermittent accumulator-head machines. The grade is characterized by a melt flow rate of 0.30–0.40 g/10 min under 190°C and 2.16 kg (ISO 1133-1:2022) and a nominal density of 0.955–0.957 g/cm³ (ISO 1183-1:2019). Because the melt flow rate is low, parison sag is limited and layer thickness can be maintained at blow-up ratios between 2:1 and 3:1; however, the higher viscosity requires tight control of die head temperature. The melt temperature at the die head is maintained at 180–200°C, while the feed zone is kept at 160–175°C and the compression zone at 180–195°C. Mould coolant inlet is set to 8–15°C, which accelerates solidification of the pinch-off zone and reduces cycle time. Blow air pressure is set at 0.6–0.8 MPa and blow time is 10–25 s depending on container wall thickness. Parison programming is used to shift wall thickness into the sidewalls away from the pinch-off, because the pinch-off is the highest-stress zone after flash trimming. Pinch-off clearance is set to 0.10–0.35 mm; excessive clearance creates a weak weld, while insufficient clearance can cause brittle tearing at the parison pinch. In household chemical containers, the environmental stress crack resistance requirement under ASTM D1693-15 Condition B with 10% Igepal at 50°C commonly requires F50 greater than 60 h, and for aggressive surfactant formulations F50 greater than 100 h is specified. For food-contact bottles, compliance with FDA 21 CFR 177.1520 and EU 10/2011 is verified on the finished article, not on pellets alone. Production-scale failures on shuttle lines are usually observed as die-lane weld lines, parison curl at the die exit, and ovality caused by insufficient mould venting; die-lane weld lines are reduced by adjusting melt temperature and die gap, while ovality is corrected by increasing mould clamp pressure and verifying vent slots at the parting line.

    What Melt Viscosity Window Governs High-Speed Injection Moulding of HDPE 5000S?

    The 5000S grade is processed on high-speed reciprocating-screw injection moulding machines with L/D ratios of 22:1–25:1 and compression ratios of 2.5:1–3.5:1. Its nominal melt flow rate of 0.8–1.0 g/10 min (ISO 1133-1:2022) places it above HDPE blow moulding grades but below low-viscosity injection grades used for small closures, thereby keeping injection pressure high enough for thin-wall pails and totes without producing excessive melt turbulence. The melt temperature window is 180–230°C, with the lower limit defined by incomplete packing and the upper limit by gate blush, odour generation, and excessive sink formation. Mould wall temperature is held at 10–30°C; lower temperatures improve cycle time but can freeze the flow front prematurely in wall sections thinner than 1.5 mm. Peak injection pressure is set at 70–100 MPa, and packing pressure is maintained at 50–70% of the injection peak, with packing time 5–12 s selected to hold gate seal. Clamp force per projected area is typically 3–6 kN/cm², and vent depths at the parting line are kept below 0.025 mm to avoid flash while allowing gas exit. Mould shrinkage for HDPE 5000S after 24 h is in the range 0.015–0.040 mm/mm (ASTM D955-21) depending on wall thickness and gate design; thick bosses and rib intersections generate higher sink. In thin-wall pails with a flow length to wall thickness ratio above 250:1, if the lot MFR drifts below 0.8 g/10 min, short shots and gate blush appear on fast-cycle lines. If the MFR rises above 1.0 g/10 min, low-temperature impact toughness measured by ISO 179-1:2010 can fall below the specification for cold-storage containers. The following table summarizes typical class data for the two grades; lot-specific certificates may differ.

    Typical class data for Sinopec Zhongke HDPE 5000S and 5502
    ParameterTest MethodHDPE 5000SHDPE 5502
    Melt flow rateISO 1133-1:20220.8–1.0 g/10 min0.30–0.40 g/10 min
    Nominal densityISO 1183-1:20190.952–0.956 g/cm³0.954–0.958 g/cm³
    Tensile yield stressASTM D638-14 / ISO 527-2:201224–27 MPa25–28 MPa
    ESCR, F50, Condition B, 10% IgepalASTM D1693-1520–40 h60–120 h

    Processing of 5000S for pails and crates is not interchangeable with 5502 without adjusting melt temperature and injection profile. On high-speed pail lines with wall thickness between 1.2 mm and 2.5 mm, the transition from 5502 to 5000S requires a reduction in melt temperature of 10–20°C and an increase in injection velocity to avoid premature freeze-off at the gate. The lower viscosity of 5000S also improves filling of rib corners and allows shorter packing time, but the mould must be designed with sufficient venting because the faster flow front can trap gas and create burn marks at the end of fill.

    Closure and cap moulding from HDPE 5000S imposes tighter organoleptic and dimensional boundaries than open-top thin-wall containers. A multi-cavity hot-runner mould with valve-gate nozzles is typically used; gate diameter is 0.5–1.5 mm, melt temperature is 190–210°C, and cooling time is 4–8 s for closures in the 3–8 g range. Thread diameter tolerance is held to ±0.15 mm and ovality below 0.30 mm to maintain seal integrity; these dimensions are measured after 24 h of conditioning at 23°C and 50% RH. Residual stress at the gate region, if not relaxed, can initiate environmental stress cracking when closures are exposed to fatty food simulants or detergent solutions; ESCR is therefore evaluated under ASTM D1693-15 Condition B in 10% Igepal at 50°C. Organoleptic requirements for food-contact closures made from 5000S require low odour and taste transfer; converters commonly conduct sensory panels after extraction in distilled water at 60°C for 24 h, while compliance is anchored to FDA 21 CFR 177.1520 and EU 10/2011. Because HDPE stress relaxation can reduce back-off torque, sealed closures are conditioned at 40°C for 24 h before torque release is measured. Published data for this specific closure configuration is limited; therefore, converter trials on the target mould are required to establish the acceptable processing window.

    When Parison Pinch-Off Integrity Governs Heavy-Duty Container Performance

    When the target container must survive drop impacts at low temperature and maintain environmental stress crack resistance after chemical exposure, extrusion blow moulding from HDPE 5502 is preferred over lower-viscosity injection grades. The moulded part is produced on an accumulator-head machine; the accumulator volume is selected between 5 L and 20 L for containers from 20 L to 1000 L. Die gap at the accumulator lips is set at 4–10 mm, and parison programming adjusts wall thickness over 40–100 positions depending on the control system. Melt temperature is held at 190–210°C with a tolerance of ±5°C at the head; excursions beyond this band create parison sag instability and weld-line thinning at the pinch-off. Mould clamp force on large parts is typically above 2000 kN depending on projected area; insufficient clamp force leads to flash at the parting line and increases the risk of blow-out at the pinch-off. The pinch-off zone is designed to compress the parison into a weld bead with thickness 0.10–0.35 mm; if the bead is too thick, trimming leaves a sharp notch that initiates low-temperature failure. If the bead is too thin, leakage occurs along the parting line. Drop impact is tested at -18°C under ASTM D2463-15, and dangerous goods packaging is qualified under 49 CFR Part 178 for UN-rated containers. ESCR after chemical exposure is evaluated under ASTM D1693-15 Condition B in 10% Igepal; industrial specifications for agricultural chemicals and automotive coolants often require F50 above 100 h. Published drop-height data for this specific configuration is limited; UN drop tests require pass heights based on filling density and container capacity.

    Melt Filtration and Additive Masterbatch Dispersion in HDPE 5000S and 5502

    Across extrusion lines running HDPE 5000S and 5502 with in-line colour concentrates, UV stabilizer masterbatches, or processing aids, melt filtration is used to remove agglomerates and incidental contamination. Screen packs are staged from 40 mesh to 120 mesh, corresponding approximately to aperture sizes of 0.38 mm to 0.125 mm; the pressure differential across the screen pack is limited to 20–25 MPa because higher differentials indicate gel accumulation and can raise melt temperature by viscous heating above 5°C. Such overheating can create oxidation gels in HDPE and reduce ESCR. Masterbatch let-down ratio is typically 2–4 wt% for colour concentrates and 1–2 wt% for UV stabilizer packages; the resulting melt flow rate shift is kept below 10% (ISO 1133-1:2022). Carbon black dispersion in polyethylene can be assessed by ISO 18553:2002, Method A, in which a compression-moulded plaque is examined for agglomerates; acceptance limits are defined in the relevant product standard, and no agglomerate larger than 0.50 mm is generally acceptable for exposed surfaces. Titanium dioxide and coloured masterbatches are checked by pressure-rise measurement across the screen pack and by optical microscopy on 50 µm sections. Although HDPE is not hygroscopic in the bulk, surface moisture at storage relative humidity above 60% can generate splay and surface pitting; conveying air is dried to a dew point below -40°C on production lines.

    Regrind and post-industrial rework streams introduce viscosity drift and contamination risk that affect both HDPE 5000S and 5502. Reworked HDPE from edge trim, start-up scrap, and rejected containers is granulated, densified, and blended with virgin pellets at 20–40 wt%; the allowable ratio is established by melt flow rate drift less than 10% from the virgin lot and ESCR retention above 80% of the virgin value under ASTM D1693-15 Condition B. Metal contamination from granulator wear or conveying equipment is controlled with magnetic traps rated for 10,000 gauss and by periodic screen pack inspection. Multiple heat cycles shift melt flow rate upward and can broaden molecular weight distribution; therefore, rework streams are tested after every 24 h of production for MFR (ISO 1133-1:2022) and for gel content on cast film or compression-moulded plaques. In blow moulding of HDPE 5502, rework above 40 wt% can degrade parison melt strength and pinch-off toughness, even if MFR remains within specification. In injection moulding of HDPE 5000S, rework above 40 wt% can increase warp due to changes in crystallinity and molecular weight distribution. A single-screw extruder with L/D ratio 25:1 and vacuum venting at -0.08 MPa is commonly used to re-pelletize rework before blending; vent vacuum below this level can leave residual volatiles that cause splay in the finished article.

    Assessing Food-Contact Compliance and Recyclability for HDPE 5000S and 5502

    For food-contact applications, the regulatory status of HDPE 5000S and 5502 is not determined by the grade name alone; converters must verify lot-specific certificates of compliance from the resin producer, additive package composition, and migration test results on the finished article. The base olefin polymer is covered by FDA 21 CFR 177.1520 when the finished article meets extraction limits for the intended food type. Under EU 10/2011, the overall migration limit for plastic food-contact materials is 10 mg/dm² for food simulants, and specific migration limits for additives and catalyst residues are declared in Annex II. In China, GB 4806.7-2016 applies to food-contact polyethylene and establishes sensory requirements, total migration, and specific migration thresholds. Recyclability is assessed in the HDPE bottle recycling stream; HDPE is coded as resin identification code #2 under ASTM D7611-19, and unpigmented or lightly pigmented HDPE 5000S and 5502 containers are generally compatible with high-density polyethylene bottle reclaim streams. The presence of metallic closures, silicone gaskets, oxygen barrier coatings, or adhesive label systems modifies recyclability and should be evaluated under the relevant plastic recycling scheme.

    Compliance checklist for HDPE 5000S and 5502 food-contact packaging
    Standard / RegulationTest Designation / ClauseRelevant Parameter
    FDA 21 CFR 177.1520Olefin polymersFood-contact clearance for HDPE homopolymer
    EU 10/2011Annex I and Annex IIOverall migration limit 10 mg/dm²
    GB 4806.7-2016National food safety standardSensory, total migration, specific migration
    ASTM D7611-19Resin identification code #2HDPE recycling stream classification
    Free Quote

    Competitive Sinopec Zhongke HDPE 5000S / 5502 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    The Sinopec Zhongke high-density polyethylene grades 5000S and 5502 occupy adjacent positions in the ethylene polymerization slate but are directed to different conversion processes. Supplier technical literature describes 5000S as a film-extrusion resin with a nominal melt mass-flow rate of 0.9 g/10 min at 190 °C under 2.16 kg load per ISO 1133-1 and a density of 0.954 g/cm3 per ISO 1183-1. Grade 5502 is specified with a nominal melt mass-flow rate of 0.35 g/10 min and a density of 0.955 g/cm3 under the same standards. The lower melt flow of 5502 corresponds to a higher average molecular weight and greater parison hang time, while the higher flow of 5000S reduces extrusion head pressure and energy draw in thin-film conversion. Both grades are supplied as free-flowing granules; the specific additive package is not detailed in every public datasheet, and batch-level confirmation should rely on the certificate of analysis.

    Material Identity and Specification Framework

    The values in Table 1 are typical declarations from supplier technical literature; they are not specification limits and should not be used as the sole basis for tooling design. The melt mass-flow rate is not an inherent viscosity; it is a single-point measurement at low shear and does not capture the full molecular-weight distribution.

    Table 1: Comparative typical properties of 5000S and 5502
    PropertyTest method5000S5502
    Melt mass-flow rate, 190 °C / 2.16 kgISO 1133-10.9 g/10 min0.35 g/10 min
    DensityISO 1183-10.954 g/cm30.955 g/cm3
    Tensile yield stressISO 527-222 MPa26 MPa
    Elongation at breakISO 527-2600 %500 %
    Vicat softening temperature A50ISO 306123 °C124 °C

    Bulk density, pellet geometry and additive concentration influence feeding stability on grooved-feed extruders. Typical bulk density for high-density polyethylene pellets is in the range 0.57–0.62 g/cm3 per supplier handling sheets; a starve-fed screw operating with level sensors should maintain hopper discharge temperature below 45 °C to avoid pellet bridging. Both grades are routinely processed with breaker-plate screen packs of 80/120/80 mesh. A pressure rise greater than 5 MPa across the screen pack at constant output indicates gel or carbon contamination; the screen pack should be replaced before pressure exceeds 8 MPa to avoid plate deflection and melt leakage.

    Capillary rheometry on a 20 mm barrel with L/D 30:1 at 190 °C typically ranks the shear viscosity of 5000S below that of 5502 across apparent shear rates from 100 s-1 to 1000 s-1. This ranking is inferred from the ISO 1133-1 melt flow values; published rheograms for the Zhongke-specific formulations are limited. The practical consequence is that 5000S can be drawn to thinner film at lower head pressure, while 5502 requires higher torque and generates greater melt-temperature rise through viscous dissipation. On a 65 mm grooved-feed extruder with 30:1 L/D, a transition from 5000S to 5502 at the same output may require 10–20 % more specific drive energy; exact machine-specific values depend on screw design and back pressure.

    Why Does 5502 Maintain Parison Integrity Longer Than 5000S?

    The difference in parison stability is measured through hang-time trials on shuttle blow-moulding equipment. In a typical trial on a machine with 50 mm screw diameter and 24:1 L/D, a 250 mm parison length at 180 °C melt temperature may show neck-in and sag thresholds at 4–6 s for 5000S and 8–12 s for 5502; published data for this specific configuration is limited, but the trend is attributable to higher melt viscosity and elasticity of the lower-flow grade. The higher molecular weight of 5502 also raises environmental stress crack resistance. Supplier literature lists F50 values above 100 h per ASTM D1693-B in 100 % Igepal CO-630 at 50 °C for 5502; comparable public data for 5000S are less consistent and should not be used without a certificate of analysis. This is the primary selection criterion for aggressive liquid-contact packaging.

    Slow crack growth resistance is not a single point property. Conversion of tensile yield stress to ESCR performance requires testing under ASTM D1693-B conditions with notched specimens immersed in an undiluted nonylphenoxy poly(ethyleneoxy) ethanol solution at 50 °C; the test records the F50 failure time. In blow-moulded containers, the pinch-off weld and wall-thickness distribution are common failure origins before bulk resin ESCR is reached. Production-scale observations on shuttle machines show that pinch-off weld flash must be trimmed cleanly; if flash thickness exceeds 0.5 mm, the weld line can become the dominant crack-initiation site. Mould cooling in the pinch-off zone should hold the steel temperature below 20 °C to solidify the weld before demoulding.

    Blown-Film Extrusion of 5000S

    Film conversion of 5000S is typically performed on single-screw extruders with grooved-feed sections and screw diameters between 45 mm and 75 mm, L/D ratios from 25:1 to 30:1. The die gap is set at 1.2–2.0 mm, and the blow-up ratio is normally held between 2.0:1 and 3.5:1. Melt temperatures at the adapter and die are maintained at 190–220 °C; temperatures below 175 °C may produce sharkskin melt fracture at apparent wall shear rates above 400 s-1. When the die gap is reduced below 1.2 mm, the shear stress at the die lip increases and surface defects propagate downstream into the frost line; raising the die temperature in 2 °C steps or lowering output is the standard corrective action. The mechanical properties of thin film are evaluated per ISO 527-3 for tensile behaviour and ISO 7765-1 for dart impact. Film thickness tolerance is typically controlled to ±5 % at 20–50 µm, with gauge variation above ±7 % associated with bubble instability.

    The draw-down ratio, defined as the ratio of die gap to final film thickness, is commonly kept between 20:1 and 60:1. If the ratio exceeds 60:1, the film may exhibit splitty behaviour in the machine direction when measured by Elmendorf tear per ISO 6383-2. To maintain balanced tear properties, the blow-up ratio and draw-down ratio are adjusted together; a blow-up ratio of 2.5:1 with a draw-down ratio of 40:1 is a typical starting point.

    Gauge variation in blown film is not solely a resin property. On a 65 mm grooved-feed extruder producing 30 µm film at 100 kg/h, bubble instability is observed when the frost line height falls below 400 mm or when the blow-up ratio exceeds 3.5:1. The operator response is to raise the cooling-air volume or adjust the iris stabilizer; no change in resin grade will correct an unstable bubble if the die lip is damaged or the air ring is uneven. Published data for this specific configuration is limited, but the operating window is consistent with general blown-film high-density polyethylene practice.

    If Blow Moulding Shot Weight Varies Beyond ±2%

    Continuous-extrusion and accumulator-head blow moulding of 5502 require closed-loop control of parison weight. On a shuttle machine with 250 kN clamp force and single-cavity tooling, shot weight variation above ±2 % typically originates from melt temperature drift, accumulator head pressure fluctuation, or parison programming errors. Head pressure changes of 2 MPa or more at constant screw speed are sufficient to alter parison wall thickness by 0.2 mm; the corrective sequence is to reduce screw speed until the pressure stabilizes, then adjust the die gap program to maintain the target weight. Melt temperature for 5502 is normally kept at 180–210 °C; exceeding 220 °C can reduce parison hang time and raise the risk of draw-down in deep-draw containers. The mould temperature is commonly held at 10–30 °C, with the pinch-off zone below 20 °C to expedite weld solidification.

    The parison die gap for 5502 is usually set at 1.0–3.0 mm, with die swell values of 15–35 % depending on melt temperature and barrel residence time. If die swell exceeds 35 %, the parison diameter may contact the mould splash plate before mould closing; the usual correction is to raise melt temperature by 2–3 °C or reduce the die gap.

    Compared with other HDPE grades in the same conversion slate, 5000S and 5502 occupy low-flow, high-melt-strength positions. They are not intended for cast film or thin-wall injection moulding. A cast-film grade with melt mass-flow rate 2.0–4.0 g/10 min may offer better draw and lower specific energy, while an injection-moulding grade with 20 g/10 min or higher offers shorter filling time. The selection between 5000S and 5502 is therefore a choice between film drawability and container durability, not a substitution for a general-purpose grade. Producers running 5000S in thin film may not obtain stable parison formation on blow moulding without grade change; similarly, 5502 may be too viscous for high-output cast-film lines.

    Compliance Matrix and Extractable Limits

    The compliance status of the final article depends on conversion and additives; the supplier resin declaration alone does not establish finished-article compliance. The following matrix lists common regulatory references applicable to unfilled high-density polyethylene.

    Table 2: Typical regulatory matrix for unfilled HDPE grades
    ReferenceScopeDocumentation basis
    FDA 21 CFR 177.1520Olefin polymers for food contact; melt index, density, extractablesSupplier food-contact letter required
    EU Regulation (EC) No 10/2011Overall migration limit 10 mg/dm²; specific migration of additivesFinished-article migration testing
    REACH Regulation (EC) No 1907/2006SVHC content, Annex XVII restrictionsSafety data sheet and supplier declaration
    RoHS Directive 2011/65/EULead, mercury, cadmium, hexavalent chromium, PBB, PBDESupplier analytical data

    Incoming quality control on a conversion line should check melt flow per ISO 1133-1 and density per ISO 1183-1 against the certificate of analysis. A deviation in melt flow of more than ±0.1 g/10 min for 5000S or ±0.05 g/10 min for 5502 may be sufficient to alter film gauge or parison weight control. The supplier documentation should include lot-specific melt flow, density, ash content and tensile yield values. Published data for the complete additive and molecular-weight distribution of these specific grades is limited; finite-window processing trials are required before locking tooling and cycle parameters.

    Storage and handling limitations for both grades are common to polyolefin resins. Pre-drying is not required for dry ambient storage; if granules are moved from cold storage into a humid processing bay, 4–8 h residence before hopper loading is recommended to prevent surface condensation. The resins should not be processed with amine-based antistatic additives or halogenated flame retardants without evaluating the stabilisation package; published data for this specific grade combination is limited. Processing temperatures should not exceed 260 °C to avoid thermal degradation on standard extrusion equipment, and the re-extruded regrind fraction should not exceed 20 % for food-contact film without specific migration testing.

    Top