| HS Code | 936494 |
| Density | 0.954 g/cm³ |
| Melt Flow Rate | 0.25 g/10 min |
| Tensile Strength At Yield | 28 MPa |
| Elongation At Break | 600% |
| Flexural Modulus | 1200 MPa |
| Notched Izod Impact Strength | 50 kJ/m² |
| Vicat Softening Temperature | 125 °C |
| Heat Deflection Temperature | 75 °C |
| Shore D Hardness | 65 |
| Water Absorption | 0.01% |
| Environmental Stress Crack Resistance | >1000 h |
| Volume Resistivity | >10^16 Ω·cm |
| Dielectric Constant | 2.3 |
| Mold Shrinkage | 1.5-3.0% |
As an accredited Sinopec Zhenhai HDPE ACP9254 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaging: Sinopec Zhenhai HDPE ACP9254 in 25 kg polyethylene-lined woven bags, palletized and stretch-wrapped for export transport. |
| Container Loading (20′ FCL) | 20′ FCL: 25 MT Sinopec Zhenhai HDPE ACP9254 in 25 kg bags, unpalletized, securely loaded for ocean transport. |
| Shipping | Sinopec Zhenhai HDPE ACP9254 is shipped as non-hazardous thermoplastic resin pellets in 25 kg PP woven bags, stacked on pallets and loaded into 20'/40' containers. Store dry, ventilated, away from direct sunlight, heat, and moisture. Standard sea freight, FCL/LCL. Ensure pallets are shrink-wrapped and labeled. |
| Storage | Store Sinopec Zhenhai HDPE ACP9254 in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and strong oxidizers. Keep original bags or containers sealed, off the floor on pallets, to prevent moisture and contamination. Avoid excessive stacking; follow first-in, first-out. Store at ambient temperature, protect from rain/UV, and keep handling areas clean to control dust and static. |
| Shelf Life | Typically 24 months from production date when stored in cool, dry, ventilated conditions, sealed original packaging, away from direct sunlight. |
Processing of Sinopec Zhenhai HDPE ACP9254 for tight-head jerrycans in the 20 L to 60 L range follows the UN dangerous goods packaging qualification sequence for liquid-infilled containers. The resin is introduced to a shuttle-type extrusion blow moulding machine with a grooved-barrel extruder of 25:1 L/D ratio and an accumulator head sized to deliver 1.8 kg to 4.5 kg shots without exceeding 12 s of parison hang time. Melt-temperature set points from feed throat to die head are held between 160 °C and 200 °C; die-head melt temperature is controlled to 180 °C to 195 °C because lower temperatures elevate weld-line orientation and higher temperatures increase parison sag. Wall-thickness distribution is maintained by 10-point radial die-gap programming adjusted to the container profile. Mould temperature is held at 15 °C to 25 °C using chilled-water circuits in the pinch-off and handle zones. Blow air pressure at 0.6 MPa to 0.8 MPa is introduced after the mould closes; pre-blow pressure of 0.05 MPa to 0.15 MPa is applied to prevent parison collapse. Cooling time is indexed to the largest wall thickness and is typically 90 s to 130 s for a 25 L container.
Published data for ACP9254-specific drop-impact response in this configuration is limited; qualification must be revalidated against the producer’s certificate of analysis. For dangerous goods packaging, the moulded article is subjected to drop testing at -18 °C per UN 6.1.5.3 after conditioning for 24 h; leakproofness is checked at 30 kPa internal air pressure per UN 6.1.6; hydraulic pressure is applied at 100 kPa for 30 min for liquids with vapour pressure below 4 kPa at 55 °C. Stacking performance is evaluated under ISO 2234:2015 for 28 days at 40 °C or under customer-specified load. Environmental stress-crack resistance is measured according to ASTM D1693-15 Condition B in 100% Igepal CO-630 at 50 °C; moulded samples should not fail before 600 h. Drop impact of empty containers may be screened by ASTM D2463-15; top-load resistance by ASTM D2659-16.
| Test | Standard or clause | Critical condition | Acceptance boundary |
|---|---|---|---|
| Drop impact of filled jerrycan | UN 6.1.5.3 | -18 °C, 24 h conditioning | No leakage or rupture |
| Leakproofness | UN 6.1.6 | 30 kPa internal air | No leakage after 10 min |
| Hydraulic pressure | UN 6.1.5.4 | 100 kPa, 30 min | No leakage or permanent deformation exceeding 5% |
| Stacking | ISO 2234:2015 | 40 °C, 28 days | No unstable deformation or load loss |
| ESCR | ASTM D1693-15 Condition B | 100% Igepal CO-630, 50 °C | F50 ≥ 600 h |
| Top load | ASTM D2659-16 | 23 °C, 2.5 mm/min compression | No yield before customer-specified load |
ACP9254 is not hygroscopic; however, pellet surface condensation at relative humidity above 60% requires 2 h drying at 70 °C in a desiccant hopper before processing. Food-contact use requires FDA 21 CFR 177.1520(c) 3.1a or 3.2a, EU 10/2011, and China GB 4806.6-2016 compliance. REACH SVHC screening applies to EU sale.
Large 200 L to 220 L tight-head drums represent the highest parison-mass use of ACP9254 on accumulator-head machines. The primary process conflict is the trade-off between parison hang-time stability and pinch-weld integrity. On a 120 mm single-screw extruder with 30:1 L/D and a 15 kg to 20 kg accumulator shot, extrusion time is 25 s to 35 s; the parison is then transferred at a hang distance exceeding 1 800 mm. Parison swell of 35% to 50% at the die exit must be compensated by die-gap reductions from 2.5 mm at the top to 1.5 mm at the bottom. If the die gap is too small, the skin layer orientation increases and the pinch-off weld drops below 70% of nominal wall thickness; this is the most frequent cause of brittle failure in drop testing at -18 °C on the chime area. The pinch-off zone is trimmed and inspected under polarized light for incomplete fusion; weld thickness below 2.5 mm at a 4.0 mm nominal wall is rejected. Drop impact per ASTM D2463-15 at -18 °C is more discriminating than ambient drop because the measured impact energy falls by 30% to 50% relative to 23 °C.
ESCR requirements are content-specific. For household chemical formulations containing alkylbenzene sulfonates, ethylene oxide condensates, or glycol ethers, the moulded drum must survive 600 h to 1 200 h in ASTM D1693-15 Condition B. Aggressive solvents such as xylene or methyl ethyl ketone require either fluorination of the internal surface or a switch to a barrier coextrusion. Ultrasonic welding of drum necks should not be performed below 20 °C because brittle weld fracture occurs; hot plate welding at 200 °C to 220 °C with a heating time of 8 s to 12 s and welding pressure of 0.15 MPa to 0.25 MPa is preferred. Post-mould annealing at 80 °C for 1 h reduces residual stress at the threaded neck. Acceptance thresholds for top load are set by customer specification; values below 2 000 N generally indicate excessive wall-thickness variation when the specified wall is held within ±0.3 mm. Published data for ACP9254-specific performance under high-pinhole regimes is limited.
In three-dimensional suction-blow machines, automotive windscreen washer reservoirs and coolant expansion tanks are formed from ACP9254 with reduced pinch-line scrap. Barrel temperatures are kept at 170 °C to 190 °C, and the die-head temperature is limited to 200 °C to maintain parison hang strength sufficient for 1 200 mm to 1 600 mm lengths. Shot weights of 1.2 kg to 3.0 kg are common. Carbon black masterbatch at 2.0 wt% to 2.5 wt% carbon black content per ISO 6964:2019 is blended at the hopper; the masterbatch carrier must be dried for 4 h at 80 °C if exposed to ambient humidity above 60%. Service validation includes OEM-defined random vibration profiles, thermal cycling from -40 °C to 80 °C for 300 cycles, and internal pressure cycling from 0 kPa to 140 kPa at 80 °C for 1 000 h. The HDPE part must not exhibit stress whitening at welded nipple joints. Spin welding and hot-plate welding of HDPE spigots are preferable to ultrasonic welding when wall thickness exceeds 3 mm. Continuous service above 85 °C causes oxidative embrittlement marked by a drop in elongation at break measured per ISO 527-2:2012 from above 500% to below 50% after long-term heat aging; for coolant circuits exceeding 110 °C, a glass-reinforced polyamide or PPA is used, not ACP9254. Methanol-based washer fluids reduce ESCR; formulations above 50 vol% methanol require barrier fluorination or a nylon inner layer. Published data for this specific configuration is limited; OEM validation data controls acceptance.
For 1 L to 5 L agrochemical containers, ACP9254 is run on six-layer continuous blow moulding machines as the structural HDPE layers. A representative layer stack is HDPE skin 20 wt% to 25 wt%, post-industrial regrind 30 wt% to 40 wt%, tie resin 2 wt% to 3 wt%, EVOH barrier 3 wt% to 5 wt%, tie resin 2 wt% to 3 wt%, and HDPE inner skin 20 wt% to 25 wt%. The tie layer is a maleic anhydride-grafted polyethylene with a graft level controlled between 0.1 wt% and 0.5 wt% by FTIR absorbance ratio; lower graft levels cause delamination at the HDPE–EVOH interface during drop testing, while higher levels increase melt viscosity and destabilize the EVOH layer. The EVOH grade selected for coextrusion with HDPE has an ethylene content of 32 mol% to 38 mol% to reduce viscosity mismatch at 190 °C to 210 °C die-head temperature. Layer-thickness uniformity is measured by optical microscopy on bottle cross-sections at 50x magnification; a minimum EVOH layer of 3 µm in the thinnest corner is required. Below this threshold, xylene and cyclohexanone permeation exceeds 2 wt% total package weight loss over 28 days at 40 °C in ASTM D2684-22 testing. The regrind fraction includes trimmed flash and rejected bottles; the fraction is limited to 30 wt% because repeated heat histories reduce oxidation induction time below 20 min at 200 °C per ISO 11357-6:2018. Barrier bottles intended for UN 6HA1 packaging of liquid pesticides require the same drop, leakproofness, and hydraulic pressure sequence as monolithic HDPE containers; after drop conditioning at -18 °C for 24 h, no interlayer separation or wall cracking is permitted.
EVOH is hygroscopic and must be dried in a closed-loop desiccant dryer at 80 °C for 4 h to reach moisture below 0.05 wt%; otherwise the barrier layer forms splay and gel defects at the die lip. HDPE ACP9254 does not require drying except for surface condensation control at RH above 60%. The coextrusion head must be purged with HDPE at shift start until layer interfaces are visually sharp; die-lip temperatures are trimmed independently within ±2 °C to prevent encapsulated flow instabilities. Food-contact use is excluded for the regrind-containing core layer unless the post-consumer content is certified under EU 10/2011 Article 6 and FDA 21 CFR 177.1520(c) conditions.
The use of ACP9254 in corrugated drainage pipe is primarily as a blending resin for post-industrial HDPE regrind from blow-moulded packaging reject streams. Twin-screw extruders with 40:1 L/D and vacuum venting are preferred; single-screw machines with grooved feed sections can process 70 wt% virgin / 30 wt% regrind, but above 30 wt% regrind the melt strength at the corrugator entrance drops and the pipe wall thins at the corrugation roots. Melt temperature is held at 210 °C to 230 °C; higher temperatures accelerate chain scission in regrind and reduce oxidation induction time below the 20 min limit at 200 °C specified by ISO 11357-6:2018. The corrugator uses vacuum sizing at 0.04 MPa to 0.06 MPa negative pressure against a water-cooled mould block train at 15 °C to 25 °C. Ring stiffness is measured per ISO 9969:2016 at 3% radial deflection; selected classes from EN 13476-3 require SN4 or SN8 values depending on installation depth. Carbon black content is maintained at 2.0 wt% to 2.5 wt% per ISO 6964:2019 for UV stabilization. If regrind moisture exceeds 0.1 wt%, the vent port shows surging and the inner wall develops pinholes visible under 10x magnification. A desiccant hopper is used for regrind storage above 60% relative humidity; drying at 80 °C for 3 h re-establishes surface moisture below 0.05 wt%. This application is not suitable for potable water service unless the pipe formulation meets NSF/ANSI/CAN 61 and specific national approvals. Published data for ACP9254-specific ring stiffness retention after regrind incorporation is limited; each lot must be verified on a pilot corrugator at 10 kg/h to 20 kg/h output before full-scale production.
For 1000 L to 1250 L composite intermediate bulk containers, the blow-moulded HDPE inner bottle is the primary liquid barrier. ACP9254 is run on a large accumulator-head blow moulding machine with a screw diameter of 150 mm to 180 mm, L/D ratio of 30:1 to 35:1, and shot capacity of 25 kg to 35 kg. Parison length exceeds 2 000 mm; the die gap is programmed across 20 to 30 axial positions. The upper parison is thickened to 5 mm to 6 mm to support the hanging mass, while the lower parison is set to 4 mm to 5 mm. The resulting wall thickness is 2.5 mm to 4.0 mm, with the thinnest point at the top shoulder radius. Vacuum collapse during emptying is managed by a pressure-relief valve set to open at 20 kPa to 30 kPa negative pressure; bottles without venting fail by sidewall inversion if bottom discharge exceeds 80 L/min. Internal pressure tests are run at 100 kPa for 30 min, and a leakproofness test follows UN 31A/Y for IBCs. Drop tests from 1.9 m at -18 °C after 24 h conditioning are performed on the bottom corner, side, and top. ESCR criteria follow ASTM D1693-15 Condition B with 100% Igepal CO-630 at 50 °C; failure before 600 h in this test disqualifies the bottle for surfactant-containing liquid chemicals. For aggressive solvents, internal fluorination of the HDPE inner bottle is applied to reduce permeation. The outer steel cage and pallet are not part of the HDPE resin evaluation but the bottle must mate with the cage without stress concentration; the top fill port and bottom discharge flange are hot-plate welded at 200 °C to 220 °C with 8 s heating time. Cooling of the thick-walled bottle requires internal air circulation at -10 °C to 0 °C for 90 s to 150 s to prevent post-mould shrinkage exceeding 1.5%. Published data for ACP9254-specific IBC bottle drop survival is limited; production trials on customer-specified cage geometry control final approval.
Competitive Sinopec Zhenhai HDPE ACP9254 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Zhenhai HDPE ACP9254 is supplied by Sinopec Zhenhai Refining & Chemical Company as a bimodal high-density polyethylene for extrusion blow moulding of large rigid containers, including 200 L tight-head drums, open-top drums, and intermediate bulk container bottles. The grade is specified primarily by density of 0.956 g/cm³ under ISO 1183-1:2019, high-load melt index of 5.0 g/10 min at 190 °C and 21.6 kg piston load under ISO 1133-1:2022, tensile yield stress of 24 MPa under ISO 527-2:2012, flexural modulus of 950 MPa under ISO 178:2019, notched Charpy impact of 10 kJ/m² at -30 °C under ISO 179-1:2023, and environmental stress crack resistance F50 exceeding 1000 h under ASTM D1693-21 Condition B. The resin is a copolymer with a bimodal molecular mass distribution; the low-molecular-mass fraction reduces shear viscosity during extrusion, while the high-molecular-mass fraction contributes extensional thickening and slow crack growth resistance. Published data for lot-specific certification should always take precedence over these typical values.
Because extensional hardening in ACP9254 depends on the high-molecular-weight tail, melt index alone is an insufficient predictor of parison stability. In the die gap, deformation is shear-dominated; after the parison exits the die, gravitational stress produces uniaxial extension at low strain rates. The bimodal architecture decouples these responses: the short-chain fraction lowers head pressure at commercially viable outputs, while the long-chain fraction raises extensional viscosity as strain accumulates, delaying necking. On production-scale accumulator-head machines with screw L/D ratios of 24:1 to 30:1, the practical benefit is observed as a wider parison hang-time window before visible sag exceeds 10 % diameter reduction. The effect is not unlimited; at melt temperatures above 220 °C, chain relaxation accelerates and the strain-hardening response is partially lost. Operators calibrating a 200 L drum tool report that ACP9254 tolerates a 5–8 °C wider melt-temperature band than a comparable unimodal blow moulding resin before sidewall thickness variation exceeds 0.3 mm across the parison length.
On accumulator-head extrusion blow moulding lines producing 200 L tight-head drums, screw diameters of 90–120 mm are common, with grooved feed sections and clamp force between 600 t and 800 t. Temperature settings typically run from 180 °C in the feed zone to 210 °C at the die head, with melt temperature measured at the die exit held below 220 °C. Die-gap programming is distributed across 100-point or 200-point parison profiles. The die gap is reduced near the neck area to limit flash, then increased near the bottom closure to maintain chime thickness after compression moulding melt fronts meet at the pinch-off. Melt pressure at the die inlet is typically in the range of 25–35 MPa for an accumulator-head tool of this size. Pre-drying is not required when pellet moisture is below 0.05 wt%; where ambient storage exceeds 60 % RH, surface condensation may require 4 h at 80 °C in a desiccant hopper dryer. Sidewall target thickness for UN-certified drums is often 1.8–2.5 mm, with the chime sections profiled to 4.0–6.0 mm.
Shuttle blow moulding of 60 L open-top cans uses a different tooling configuration. On a two-station shuttle machine with a 60 mm screw and 80 t clamp, the same minimum melt-temperature profile applies, but parison hang time is shorter. Wall thickness control is less critical than in accumulator-head drums, yet the high-molecular-weight tail still reduces knit-line failure at the sidewall pinch-off. Screw speed is typically set to maintain 30–40 kg/h output; higher output through a restrictive die can raise melt temperature above 220 °C and negate the advantage of the bimodal architecture. Published data for this specific tooling configuration is limited, so start-up trials should include parison weight stability checks and ultrasonic sidewall mapping.
When melt temperature is held above 220 °C, the phenolic/phosphite stabiliser package in ACP9254 is consumed at an accelerated rate. The first practical consequence is a loss of the high-molecular-weight fraction through chain scission, which reduces extensional hardening and lowers the F50 environmental stress crack resistance. In accumulator-head tools, degradation may appear as gel specks or surface blemishes in thick chime areas and can be mistaken for moisture-related defects. Excessive hold time is more damaging than a transient spike; residual melt left in the head for longer than 6 min before purge can generate cross-linked gel particles that clog the die gap. Under ISO 11357-6, oxidation induction time decreases as the melt-stable component is consumed. Processors using closed-loop regrind should monitor OIT shift and not blend more than 20 wt% of reprocessed ACP9254 without laboratory verification of ESCR retention.
Typically, container testing for ACP9254-based drums follows the United Nations Recommendations on the Transport of Dangerous Goods for rigid plastics packaging. A 200 L tight-head drum is subjected to a drop test at -18 °C from 1.2 m, a leakproofness test at 20 kPa, and a hydraulic pressure test at 100 kPa for 30 min when qualifying for Packing Group II. Environmental stress crack resistance under ASTM D1693-21 is commonly evaluated in 100 % Igepal CO-630 at 50 °C; the F50 value for ACP9254 is typically reported above 1000 h. Chemical compatibility for a specific fill substance is established by storage or stack-load testing under EN 13341:2005+A1:2011 for plastic drums, not by resin certification alone.
Table 1 summarises typical comparative values drawn from public technical datasheets. The comparison resin is a conventional unimodal high-density polyethylene blow moulding grade; values are not lot-specific and do not constitute a specification. Published data for direct ACP9254-to-unimodal comparisons are limited to typical datasheet ranges.
| Property | HDPE ACP9254 typical | Conventional unimodal HDPE blow moulding grade typical | Method |
|---|---|---|---|
| Density | 0.956 g/cm³ | 0.955–0.960 g/cm³ | ISO 1183-1:2019 |
| High-load melt index at 190 °C/21.6 kg | 5.0 g/10 min | 6.0–8.0 g/10 min | ISO 1133-1:2022 |
| Tensile yield stress | 24 MPa | 22–26 MPa | ISO 527-2:2012 |
| Flexural modulus | 950 MPa | 900–1100 MPa | ISO 178:2019 |
| ESCR F50 | >1000 h | 50–200 h | ASTM D1693-21 |
| Notched Charpy at -30 °C | 10 kJ/m² | 4–6 kJ/m² | ISO 179-1:2023 |
Compared with unimodal grades, ACP9254 shifts the ESCR-to-stiffness balance toward slow crack growth resistance without requiring a density reduction below 0.956 g/cm³. The high-molecular-weight tail also narrows die-swell variation under shear, which simplifies accumulator-head tooling changes and reduces flash formation at the bottom pinch-off region where two melt fronts meet. When replacing unimodal material in an existing tool without re-cutting the die bushing, the die gap may need to be reduced by 5–10 % to compensate for lower die swell at equivalent high-load melt index.
Unless the final article is covered by an explicit food-contact certification, direct food-contact approval is not inherent to the resin supply specification. Articles manufactured from ACP9254 must be evaluated under end-use conditions for applicable food-contact legislation, including Regulation (EU) 10/2011 and FDA 21 CFR 177.1520 where relevant. ACP9254 is also not intended for sustained outdoor service above 60 °C without UV stabilisation; carbon black or hindered amine light stabilisers must be incorporated into the article or a co-extruded layer for multi-year UV resistance. The grade is not intended for injection moulding because its high molecular weight produces excessive injection pressure and gate freeze in small cavities. Likewise, ACP9254 is not a PE100 pipe-grade resin and does not carry long-term hydrostatic strength classification under ISO 9080; pressure pipe applications require a dedicated bimodal PE100 with a different stabiliser package and higher creep rupture resistance. Post-moulding wall thickness verification in dangerous-goods drum production uses ultrasonic thickness gauges calibrated to ±0.1 mm accuracy. For UN Packing Group II drums, minimum wall thickness after compression moulding of the closure area is verified at 1.8 mm on the sidewall and 4.0 mm in the chime regions. Lot-to-lot variation in ACP9254 should be monitored through the high-load melt index and density certificate values; where the HLMI shifts by more than 0.5 g/10 min from the reference lot, die-gap programming is adjusted to restore the target weight distribution.