Sinopec Zhenhai Hdpe 7750m2

Sinopec Zhenhai HDPE 7750M2

    • Product Name: Sinopec Zhenhai HDPE 7750M2
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 914325
    Melt Flow Rate 7.5 g/10 min (190°C, 2.16 kg)
    Density 0.950-0.955 g/cm³
    Melting Point 130-135 °C
    Tensile Strength At Yield ≥25 MPa
    Elongation At Break ≥500%
    Flexural Modulus ≥1000 MPa
    Vicat Softening Temperature ≥120 °C
    Brittleness Temperature ≤-70 °C
    Water Absorption <0.01%
    Shore D Hardness ≥60
    Mold Shrinkage 2-5%
    Volume Resistivity ≥10^16 Ω·cm
    Dielectric Constant 2.3
    Thermal Conductivity 0.4 W/m·K
    Specific Heat Capacity 1.9 kJ/kg·K

    As an accredited Sinopec Zhenhai HDPE 7750M2 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Sinopec Zhenhai HDPE 7750M2 is typically supplied in 25 kg bags, with 1000 kg jumbo bags available.
    Container Loading (20′ FCL) 20' FCL loading: Sinopec Zhenhai HDPE 7750M2 in 25kg bags, palletized, shrink-wrapped, approximately 20MT net per container.
    Shipping Sinopec Zhenhai HDPE 7750M2 is a non-hazardous high-density polyethylene resin, shipped as odorless pellets in 25 kg woven bags, jumbo bags, or bulk containers. Typical 20'FCL load: 18–20 MT. Standard export packaging. Keep dry, cool, ventilated; avoid moisture, sunlight, and ignition sources. Not classified as dangerous goods.
    Storage Store Sinopec Zhenhai HDPE 7750M2 in a cool, dry, well-ventilated warehouse, protected from direct sunlight, rain, and moisture. Keep original bags sealed on pallets, away from heat, ignition sources, strong oxidizers, and incompatible materials. Avoid prolonged UV exposure and contamination. Maintain moderate stacking heights to prevent deformation. Observe good housekeeping, local regulations, and first-in, first-out stock rotation.
    Shelf Life Sinopec Zhenhai HDPE 7750M2 typically has a 24-month shelf life when stored in original packaging under cool, dry, ventilated conditions.
    Application of Sinopec Zhenhai HDPE 7750M2

    Sinopec Zhenhai HDPE 7750M2 is a bimodal high-density polyethylene pipe-grade resin with a nominal density of 0.949 g/cm³ and melt flow rate of 0.23 g/10 min at 190 °C/5 kg. The resin is processed almost exclusively by grooved-feed single-screw extrusion into thick-wall pressure pipes; its low melt flow under 5 kg load produces high melt viscosity and controlled sag behavior during vacuum calibration, which is appropriate for large-diameter pipe but incompatible with short-cycle injection molding of thin-wall fittings. The six downstream segments below are actual PE100 pipe applications, each restricted to the resin’s qualified performance envelope. Non-pipe uses such as blown film, sheet, or high-speed profile extrusion are excluded because the molecular architecture is designed for slow crack growth resistance and hydrostatic design basis rather than melt extensibility.

    Potable water transmission pipe extrusion from 7750M2 is governed by ISO 4427-1:2007, EN 12201-1:2011, and GB/T 13663.1-2018. The PE100 classification requires the hydrostatic strength regression curve to satisfy a lower predictive limit of 10.0 MPa at 20 °C for a 50-year service life under ISO 9080:2012; lot release certificates should also record melt flow rate at 190 °C/5 kg, density, and contaminant level before conversion. In compounding, the natural pellet is dry-blended with a potable-water-approved blue or carbon black masterbatch at 2.0–2.5 wt%, with carbon black dispersion assessed by ISO 18553:2002 where black pipe is used for above-ground storage or tropical exposure. The conversion process is a grooved-feed single-screw extruder with L/D 30:1–33:1, barrier screw geometry, and barrel zones set from 180 °C to 220 °C; die head temperature is held between 200 °C and 220 °C. Vacuum sizing is performed in multi-chamber calibration sleeves at -0.3 bar to -0.6 bar, and online ultrasonic wall-thickness monitoring is configured to hold tolerance class A of ISO 11922-1:1997. Finished pipe types include SDR11 and SDR17 pressure pipes from 20 mm to 1200 mm outside diameter, supplied as coils for small diameters and straight lengths for larger diameters; all potable water products must be purged and capped to prevent contamination after extrusion.

    What Limits Rapid Crack Propagation Resistance in PE100 Gas Distribution Main Extrusion?

    Natural gas distribution main extrusion from 7750M2 is controlled by ISO 4437-1:2014, EN 1555-1:2010, ASTM D2513-17, and GB/T 15558.1-2015. The compound is prepared with a gas-pipe yellow masterbatch at 2.0–2.5 wt%; carbon black is not used because the identification regime for buried gas mains requires yellow coloration, and any pigment or additive package must not compromise the fusion bead strength when tested under the butt fusion procedures of ISO 21307:2017. Extrusion is performed on a single-screw grooved-feed line with L/D 30:1–33:1, barrel profile 190–230 °C, and die head temperature limited to 220 °C to avoid oxidative degradation; melt pressure at the breaker plate is monitored against a line-specific upper limit, typically 200–350 bar, to prevent screen pack blinding because carbon black masterbatch dispersion defects can nucleate slow crack growth. Rapid crack propagation resistance is verified by ISO 13477:2008 critical pressure testing at 0 °C, and slow crack growth resistance is verified by ISO 13479:2008 on notched pipes. Terminal products are SDR11 and SDR17.6 gas mains from 20 mm to 630 mm outside diameter, with coils produced up to 125 mm and straight lengths produced at 6 m or 12 m; electrofusion fittings are produced from a separate higher-MFR PE100 compound because the 0.23 g/10 min melt flow rate of 7750M2 causes excessive pressure drop and short-shot risk in injection molding.

    In closed-loop geothermal ground heat exchanger construction, the low melt flow and high slow crack growth resistance of 7750M2 support production of SDR11 U-bend loops and header lines from 32 mm to 63 mm outside diameter. Governing pipe standards include ISO 4427-1:2007, ASTM D3035-22, and CSA B137.1-17 where applicable to buried pressure water service. The formulation uses 2.0–2.5 wt% carbon black masterbatch for UV resistance during outdoor storage; lot acceptance includes melt flow rate at 190 °C/5 kg, density, and oxidation induction time where required by the geothermal loop installer specification. Processing is carried out on a grooved-feed extruder with barrel temperatures 180–220 °C, followed by vacuum calibration with closed-loop water temperature held at 15–25 °C to minimize residual stress and pipe bow. Socket fusion is performed at heater plate temperature 200–220 °C with fusion pressure and time settings per the fitting manufacturer’s parameters; after loop assembly, the circuit is pressure-tested at 1.5 times the nominal operating pressure for 1 h. Finished product types include vertical borehole U-bend loops, horizontal trench slinky loops, and supply/return headers in 32 mm, 40 mm, 50 mm, and 63 mm SDR11 dimensions. Compatibility with glycol/water heat transfer fluids must be confirmed with the fluid supplier; published data for this specific resin and fluid combination is limited, so no universal maximum glycol concentration is assigned without immersion testing.

    Compliance and formulation matrix for HDPE 7750M2 downstream scenarios
    ScenarioPrimary standardsMasterbatch addition ratioFinished pipe range
    Potable water mainsISO 4427-1:2007, EN 12201-1:2011, GB/T 13663.1-20182.0–2.5 wt%20–1200 mm OD
    Gas distribution mainsISO 4437-1:2014, EN 1555-1:2010, ASTM D2513-172.0–2.5 wt% yellow20–630 mm OD
    Geothermal loopsISO 4427-1:2007, ASTM D3035-22, CSA B137.1-172.0–2.5 wt% carbon black32–63 mm OD
    Industrial effluentsISO 4427-1:2007, EN 12201-1:2011, ASTM F714-132.0–2.5 wt% carbon black110–1600 mm OD

    When Dilute Acidic Effluent Lines Require PE100-Rated Slow Crack Growth Resistance

    Industrial pressure piping for aqueous effluents, mine dewatering, and chemical plant service uses 7750M2 only after chemical resistance is verified against ISO/TR 10358:2005 for the specific species, concentration, and temperature. Pipe standards include ISO 4427-1:2007, EN 12201-1:2011, and ASTM F714-13, with long-term hydrostatic strength established by ISO 9080:2012 and resin classification under ASTM D3350 where procurement documents require a cell classification. The formulation is a black compound with 2.0–2.5 wt% carbon black masterbatch; for above-ground lines exposed to ultraviolet radiation, carbon black content is maintained at ≥2.0 wt% to satisfy weathering criteria for long outdoor service. The conversion route is thick-wall pressure pipe extrusion on a barrier screw with L/D 30:1–33:1, and a melt pump is used on some lines above 400 mm outside diameter to reduce extruder pulsation and wall-thickness variation. Finished pipe types include SDR17, SDR13.6, and SDR11 from 110 mm to 1600 mm outside diameter, giving pressure ratings up to 16 bar for water and selected dilute effluents. The operational boundary excludes strong oxidizers, aromatic hydrocarbons, and chlorinated solvents; concentrated acid service above 60 °C requires published chemical resistance data and elevated-temperature hydrostatic verification before production is released.

    Pressure Sewer Force Main Extrusion and Surge Fatigue Control

    Municipal sewage force mains made from 7750M2 are specified under ISO 4427-1:2007, EN 12201-1:2011, and ASTM F714-13, with hydrostatic design basis validated by ISO 9080:2012. The pipe compound is produced with 2.0–2.5 wt% carbon black masterbatch to provide UV protection during open-trench storage and to maintain consistent pipe wall density. Extrusion processing is carried out on grooved-feed single-screw lines with barrel temperatures 180–220 °C; melt temperature must remain below 230 °C to avoid thermal oxidation and gel formation that would reduce slow crack growth resistance. Force mains are produced as SDR21, SDR17, and SDR11 in outside diameters from 110 mm to 630 mm, serving gravity interceptor discharge, lift-station pressure sections, and temporary bypass lines. Surge pressure amplitude is limited to 2.0 times the steady-state working pressure unless a site-specific hydraulic transient analysis demonstrates that lower fatigue loading is present; cyclic pressure testing under the project specification is performed on finished pipe cuts to confirm butt fusion joint integrity after hydraulic shock.

    Tailing and slurry transport lines in mineral processing are another actual downstream segment where 7750M2 is converted into thick-wall HDPE pipe, with the primary governing specifications being ISO 4427-1:2007 for pressure pipe and ASTM F714-13 for outside-diameter-controlled polyethylene pipe; resin classification under ASTM D3350 is referenced in North American mining procurement. The pipe formulation contains 2.0–2.5 wt% carbon black masterbatch for outdoor stockpiling of finished pipe and for resistance to ultraviolet degradation in above-ground mineral processing installations. Processing is performed on large-bore pipe extrusion lines with grooved-feed extruders of 120–150 mm screw diameter and L/D 30:1–33:1, using vacuum calibration tanks sized for outside diameters from 200 mm to 1000 mm. Finished products include SDR11 and SDR17 tailings mains, return-water lines, and butt-fused spools fabricated in the plant or at the mine site. Abrasion resistance of 7750M2 is not characterized by a published ISO slurry abrasion test; service life under sharp, angular solids must be based on field wear allowance and wall-thickness monitoring, because published data for this specific configuration is limited.

    Free Quote

    Competitive Sinopec Zhenhai HDPE 7750M2 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Sinopec Zhenhai HDPE 7750M2 is a bimodal high-density polyethylene grade intended for pressure pipe extrusion in the PE100 class under ISO 12162. The molecular architecture combines a high-molecular-weight fraction with controlled short-chain branching, which contributes to slow crack growth resistance evaluated under ISO 13479, and a lower-molecular-weight fraction that reduces melt viscosity during single-screw extrusion. This design distinguishes 7750M2 from conventional unimodal HDPE pipe grades and from PE80 resins, which are limited to a minimum required strength of 8.0 MPa compared with 10.0 MPa for PE100 under ISO 9080. The model designation 7750M2 is a producer short name; its technical definition is set by the certificate of analysis and by pipe-system standards rather than by the grade number alone.

    Published lot-specific data for this commercial configuration is limited in public literature. Converter qualification must be based on the producer certificate of analysis. Typical acceptance tests for a PE100 pipe resin include melt flow rate under 5 kg at 190 °C according to ISO 1133-1:2022, density by ISO 1183-1:2019, tensile yield stress and elongation by ISO 6259-1:2015, and hydrostatic pressure testing by ISO 1167-1:2006. The common PE100 extrusion class generally shows a melt flow rate in the 0.20–0.30 g/10 min range and a compound density near 0.949–0.959 g/cm³; these class ranges must not be substituted for the lot-specific values of 7750M2.

    The designation PE100 does not itself define the full material specification; it defines the minimum required strength after long-term hydrostatic testing and extrapolation. To claim PE100 classification, pipe specimens must satisfy the hydrostatic strength requirements of ISO 9080:2022 and ISO 12162:2009. The short-term test points in ISO 1167-1:2006 differ from long-term extrapolation; a single burst test cannot establish PE100 status. Therefore, 7750M2 is most correctly specified by the producer certificate for melt flow rate, density, tensile properties, oxidation induction time, and the hydrostatic test programme, not by the PE100 label alone.

    In municipal potable water distribution, the resin is extruded into solid-wall pipe conforming to ISO 4427:2019. The PE100 classification permits an SDR 11 pipe to carry a PN 16 rating at 20 °C with a design stress of 8.0 MPa; the same SDR 11 dimension in PE80 carries a PN 12.5 rating because the design stress is 6.3 MPa. For a fixed pressure class, substitution of 7750M2 for a PE80 resin therefore permits a thinner wall, a larger bore at equal outside diameter, or lower mass per metre. The exact outside-diameter and wall-thickness combinations are tabulated in ISO 4065:2018 and not in the resin datasheet.

    What Processing Conditions Govern Pipe Extrusion of Bimodal PE100 Grades?

    Production-scale pipe lines for PE100 grades commonly use single-screw extruders with grooved feed sections and L/D ratios in the 30:1–37:1 range. The grooved bushing raises the effective solids-conveying angle and stabilizes throughput against die-head pressure, which is necessary when the high-molecular-weight fraction increases melt viscosity. Melt temperature at the die entry is normally controlled in the 210–230 °C window for PE100 pipe extrusion. Operation above this window accelerates consumption of the antioxidant package and lowers the oxidation induction time measured under ISO 11357-6. Operation below the optimum window increases head pressure, reduces melt homogenisation, and can generate visible gel particles at the pipe surface.

    In capillary rheometry under ISO 11443:2021, bimodal PE100 grades normally display pronounced shear thinning in the 10–1000 s⁻¹ range encountered in extruder metering sections and die land flow. The high molecular weight fraction increases the entrance pressure drop; the low molecular weight fraction lowers wall shear stress. This combination permits stable throughput at high head pressure and supports the production of large-diameter pipe. The shear viscosity at 210 °C and 100 s⁻¹ for PE100 pipe grades often lies in the 1000–2000 Pa·s range, but the lot-specific value for 7750M2 must be obtained from capillary rheometry rather than inferred from the melt flow rate alone.

    Barrier screws with dispersive mixing elements are commonly used; the screw design must limit shear heating because the high-viscosity melt can develop a substantial axial temperature rise. Melt temperature should be measured at the die land and not assumed from barrel setpoints. An increase in melt temperature of 10–15 °C above the setpoint has been observed in production lines with worn screws or restricted screens, and this can alter pressure pipe surface finish and stabilizer consumption. Replacement of screens and screw elements should follow the equipment manufacturer’s inspection interval.

    For thick-wall pipe above 25 mm wall thickness, cooling rate controls residual stress and notch sensitivity. Vacuum calibration and spray cooling tanks with water temperatures in the 15–25 °C range are typical. Raising the water temperature to 30–40 °C can improve surface gloss but may slow the cooling rate enough that the inner wall remains molten while the outer wall solidifies, producing asymmetric crystallinity and elevated shrinkage. The haul-off speed is slaved to extruder output by wall-thickness monitoring; ultrasonic gauge measurements according to ISO 3126 keep wall thickness within specified tolerances. Production trials on twin-screw lines are possible, but the shear history differs from a grooved-feed single-screw extruder and must be evaluated separately.

    If pellets are stored outdoors or exposed to relative humidity above 60%, surface condensation on cold resin can introduce moisture into the melt. A hopper dryer at 70–80 °C for 2–4 h removes surface water; polyethylene is non-hygroscopic and does not require deep-bed drying unless the silo is open to rain ingress. Avoid blending with unqualified recycled polyolefin or high-viscosity polypropylene because melt-phase separation can reduce slow crack growth resistance measured under ISO 13479. For black pipe production, carbon black masterbatch should be added in controlled proportions and then evaluated for dispersion under ISO 18553, because poor dispersion creates local stress concentrations.

    When black pipe is produced, carbon black masterbatch is normally added to a final carbon black content of 2.0–2.5 mass% for ultraviolet resistance. Dispersion is assessed under ISO 18553; a poor dispersion rating indicates carbon black agglomerates that can initiate slow crack growth. For natural pipe or indoor plumbing, this high carbon black loading is omitted, and the base resin density and stabilizer package are adjusted. Lot-specific compounding instructions from the producer must be followed because overdosing or underdosing the masterbatch changes the density and melt flow rate of the finished compound.

    Difference in Molecular Architecture from Unimodal HDPE and PE80 Resins

    The structural difference is the bimodal molecular weight distribution and the placement of comonomer. In a bimodal pipe grade, the high-molecular-weight fraction carries much of the short-chain branching and forms tie chains between crystalline lamellae; the low-molecular-weight fraction provides a lower-viscosity continuous phase during extrusion. Under sustained hoop stress, the tie-chain network resists crack initiation and slow crack propagation. Slow crack growth is evaluated by notched pipe tests under ISO 13479:2009 or by environmental stress cracking under ASTM D1693-15. A conventional unimodal HDPE may achieve adequate short-term burst strength, but it generally does not deliver the same combination of slow crack growth resistance and processability at the same wall thickness.

    Compared with a PE80 resin, a PE100 material such as 7750M2 allows a higher design stress at the same service life. The classification thresholds are shown in Table 1. The practical consequence in pipe extrusion is not a different fundamental machine setup, but a changed operating envelope for wall thickness and pressure rating. Bimodal PE100 grades tend to have higher melt strength at low shear and more shear thinning at high shear, which supports both thick-wall sag resistance and extrusion output. The exact melt flow behaviour must be measured by capillary rheometry under ISO 11443:2021 for the specific lot rather than inferred from the melt flow rate alone. The ratio of high-load melt flow rate under 21.6 kg to melt flow rate under 5 kg is commonly used as a processability index for such grades, but the acceptable ratio for 7750M2 is defined by the producer specification.

    Table 1. Comparative classification thresholds for PE100 and PE80 pressure pipe
    ParameterPE100PE80Basis
    Minimum Required Strength at 20 °C, 50 years10.0 MPa8.0 MPaISO 9080:2022
    Overall design coefficient for water supply1.251.25ISO 12162:2009
    Design stress at 20 °C8.0 MPa6.3 MPaISO 4427:2019
    SDR 11 pressure rating at 20 °CPN 16PN 12.5ISO 4427:2019

    The difference is most visible in thin-wall design: for a 110 mm outside-diameter pipe at PN 16, a PE100 material permits a smaller wall thickness than a PE80 material under the same pressure class. The exact dimensions are tabulated in ISO 4065:2018; the resin grade contributes the long-term strength, while the dimension standard defines the wall-thickness schedule.

    Hydrostatic qualification is not a single-temperature test. Under ISO 9080:2022, long-term strength is determined by testing pipe specimens at elevated temperatures and applying time-temperature superposition. A PE100 grade must demonstrate that the 20 °C, 50-year lower predictive limit is at least 10.0 MPa. The test data set must include ductile and brittle failure modes; if the regression line is dominated by a single mechanism, the extrapolation may be invalid. This is why production certificates for PE100 often report multiple ISO 1167-1:2006 stress levels and failure times rather than a single burst pressure.

    When PE100 Replaces PE80 in Municipal Water Networks, Wall Thickness and Design Stress Change

    For network operators, the substitution of 7750M2 for a PE80 resin alters pipe dimensions, pressure rating, and jointing data but not the fundamental fusion-welding requirement. Butt-fusion parameters are governed by ISO 21307:2017 and the machine manufacturer’s data; bead-up pressure, weld soak time, and cooling time are functions of wall thickness. Because the PE100 design stress is higher, a smaller wall thickness may be specified for the same pressure. This changes heat soak and cooling time but does not remove the requirement for clean, scraped pipe ends and controlled axial alignment. Electrofusion joint qualification follows the fitting manufacturer’s instructions and the corresponding system standard.

    In mining slurry and tailings transfer, the same hydrostatic design basis is often applied, but the lack of a direct slurry-abrasion clause in ISO 4427:2019 means that the abrasion allowance must be established from site-level mass-loss measurements. Published data for 7750M2 in this specific configuration is limited. If the service temperature exceeds 20 °C, the allowable operating pressure is derated according to the temperature factors in the applicable pipe system standard. Continuous exposure to strong oxidizers, aromatic hydrocarbons, organic solvents, or surfactant-bearing slurries can induce environmental stress cracking or swelling; chemical compatibility must be checked using chemical resistance data under ISO/TR 10358:2021 before lining or immersion service is considered.

    Use in natural gas distribution is not automatic from PE100 water-pipe qualification. A gas pipe system must meet ISO 4437:2014 and may be subject to additional rapid crack propagation testing under ISO 13477, depending on pipe diameter and operating pressure. Published data for 7750M2 in gas service is limited; a separate qualification dossier from the producer and the system operator is required before such use.

    Table 2. Typical laboratory verification matrix for a PE100 pipe resin
    Property or testStandard designationFunction in qualification
    Melt flow rate at 190 °C, 5 kgISO 1133-1:2022Batch grade identity and extrusion processability
    DensityISO 1183-1:2019Compound and classification verification
    Tensile yield stress and elongationISO 6259-1:2015 / ASTM D638-14Mechanical specification and lot consistency
    Hydrostatic strengthISO 1167-1:2006PE100 classification and product surveillance
    Slow crack growthISO 13479:2009Notched-pipe stress crack resistance
    Oxidation induction timeISO 11357-6Thermal stabilizer effectiveness
    Carbon black dispersionISO 18553Black compound dispersion uniformity

    Because 7750M2 is a low-MFR pipe extrusion resin, it is not intended for small injection-moulded fittings or rotomoulding. The low melt flow rate under ISO 1133-1:2022 indicates high melt viscosity; injection moulding long thin-walled fittings from this material would require elevated melt temperatures and injection pressures, and the resulting part would not match the property profile of a fitting-grade HDPE. Qualification for gaseous fuel service is not automatic; a pipe system intended for natural gas distribution must be separately evaluated under ISO 4437:2014 and the applicable national regulation. If the product is supplied as a natural resin, the converter must add the carbon black masterbatch and stabilizer package precisely to maintain long-term hydrostatic strength and weathering resistance.

    Top