| HS Code | 633372 |
| Density | 0.955 g/cm³ |
| Meltflowrate | 8.0 g/10 min |
| Tensileyieldstrength | 28 MPa |
| Elongationatbreak | 500% |
| Flexuralmodulus | 1100 MPa |
| Notchedizodimpactstrength | 50 J/m |
| Vicatsofteningpoint | 125 °C |
| Heatdeflectiontemperature | 75 °C |
| Shoredhardness | 65 |
| Meltingpoint | 130 °C |
| Waterabsorption | <0.01% |
| Volumeresistivity | >10^16 Ω·cm |
As an accredited Sinopec Zhenhai HDPE 7260 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinopec Zhenhai HDPE 7260 comes in 25 kg PP woven bags or 1,000 kg jumbo bags, suitable for bulk shipping. |
| Container Loading (20′ FCL) | 20′ FCL container loading for Sinopec Zhenhai HDPE 7260: 25 kg bags; 25 MT unpalletized or 18 MT palletized. |
| Shipping | Sinopec Zhenhai HDPE 7260 is a non-hazardous polyethylene resin, normally shipped in 25 kg PP woven bags or 500–1000 kg jumbo bags on pallets. Keep containers clean, dry, and closed; avoid moisture, direct sunlight, heat, and contamination. No special dangerous-goods documentation or handling required. |
| Storage | Store Sinopec Zhenhai HDPE 7260 in a cool, dry, well-ventilated warehouse, protected from direct sunlight, rain, moisture, heat, and ignition sources. Keep original bags sealed and palletized; avoid contact with strong oxidizers, oils, or chemicals. Observe safe stacking limits to prevent deformation, and maintain good housekeeping to avoid dust and static hazards. |
| Shelf Life | Sinopec Zhenhai HDPE 7260: stable under normal storage; keep cool, dry, away from sunlight. Typical shelf life is 12 months. |
In returnable logistics crate production, Sinopec Zhenhai HDPE 7260 is processed as a high-flow injection-moulding feedstock with a nominal melt flow rate of 6.0 g/10 min under ISO 1133-1:2022 at 190°C/2.16 kg and a density of 0.956 g/cm³ under ISO 1183-1:2019. The compound is dry-blended at 97.0 wt% virgin 7260, 2.5 wt% carbon black masterbatch carrying 40% carbon black, and 0.5 wt% hindered phenolic antioxidant masterbatch. Melt temperature is controlled at 200°C to 230°C. The mould wall is held at 10°C to 25°C; sustained wall temperatures above 35°C extend cooling time without measurable improvement in drop impact. Injection speed is profiled from 40 mm/s to 110 mm/s. Clamp force is calculated from a projected-area multiplier of 3.0 kN/cm² to 4.0 kN/cm² on a 650-tonne hydraulic press using a 22:1 L/D general-purpose screw and hot-runner valve gates. Lot-to-lot MFI variation of ±0.5 g/10 min requires packing-pressure compensation of 5 MPa to 10 MPa to hold part mass within ±0.5%. Mechanical verification follows ISO 527-2 at 23°C and 50 mm/min for tensile yield and ISO 178 for flexural modulus. Drop impact at -20°C is tested under ISO 6603-2; published data for this specific 7260 configuration are limited, but converter validation commonly targets non-brittle failure on a 2.0 mm plaque. Terminal parts include stackable dairy crates, returnable agricultural totes, and industrial distribution boxes with anti-slip base inserts.
Thin-wall delicatessen containers moulded from Sinopec Zhenhai HDPE 7260 are limited by gate blush and jetting when acceleration exceeds 120 mm/s at a gate diameter below 0.8 mm. The food-contact formulation is compounded at 99.2 wt% 7260 with 0.8 wt% sodium benzoate nucleating masterbatch. The nucleating additive reduces cycle-time-dependent post-mould shrinkage and improves top-load stiffness under ISO 604, but it also narrows the processing window. Melt temperature is maintained at 220°C to 240°C. Mould temperature is set at 15°C to 30°C. Packing pressure is held at 40 MPa to 50 MPa for 0.8 s to 1.5 s on wall sections of 0.8 mm to 1.2 mm. After 48 h conditioning at 23°C under ISO 294-4, post-mould shrinkage is measured at 1.2% to 1.8% in flow direction and 1.6% to 2.2% transverse to flow. Food-contact compliance is evaluated under FDA 21 CFR 177.1520 and EU 10/2011; the grade itself does not automatically confer approval, and overall migration of the finished part must be verified below 10 mg/dm² under EN 1186-1. Terminal parts include 500 mL to 1000 mL refrigerator-stable deli containers and matching overcap lids.
Non-carbonated screw-cap production uses Sinopec Zhenhai HDPE 7260 at 95.0 wt% with 3.0 wt% white masterbatch containing 60% titanium dioxide and 2.0 wt% slip masterbatch containing 5% erucamide in LLDPE. The compound is gravimetrically fed at the feed throat. Pre-drying is not required when sealed silo storage remains below 60% relative humidity; if surface condensation is detected, a hopper dryer at 70°C for 1.5 h is applied. Melt temperature is held at 230°C ± 5°C to prevent erucamide decomposition and off-odour generation. The moulding operation uses injection-compression stroke control with a mould temperature of 15°C to 20°C. Post-mould ovality after 24 h at 23°C under ISO 294-4 is controlled below 0.3 mm on a 38 mm closure diameter. Closure seal integrity is verified by a positive-air pressure decay test at 20 kPa for 10 s. Direct and indirect food-contact compliance follows FDA 21 CFR 177.1520 and EU 10/2011. Terminal parts include non-carbonated beverage caps, personal care flip-top closures, and edible oil lids, excluding carbonated beverage applications because the grade lacks sufficient stress-crack resistance and sealing force retention under sustained carbonation pressure cycling.
For non-hazardous chemical and paint pails, Sinopec Zhenhai HDPE 7260 is compounded at 84.5 wt% virgin resin, 12.0 wt% post-consumer HDPE recyclate with an MFI of 0.3 g/10 min to 0.8 g/10 min, 3.0 wt% colour concentrate, and 0.5 wt% LLDPE toughening additive. Recyclate addition drops the combined melt flow rate to approximately 3.2 g/10 min, requiring a melt temperature rise to 240°C to maintain knit-line strength at the handle ears. Mould temperature is set at 10°C to 30°C. Packing pressure is maintained at 60 MPa to 80 MPa for 6 s to 10 s to eliminate sink marks around the ribbed base. Drop impact for 20 L pails intended for dangerous goods is assessed under UN 1H2 open-head plastics container requirements, with conditioning at -18°C for 48 h and a drop height of 1.8 m. Environmental stress crack resistance is measured under ASTM D1693-15 Method B in 10% Igepal CO-630 at 50°C; if the 12 wt% recyclate blend falls below 24 h, the LLDPE fraction is increased to 1.0 wt% and verification is repeated. The compound is not recommended for prolonged oxidising chemical storage above 50°C because oxidative embrittlement may occur. Terminal parts include paint pails, detergent pails, and non-hazardous chemical buckets with tamper-evident lids.
| Application | Standard or code | Test condition | Control target |
|---|---|---|---|
| Logistics crate | ISO 527-2 | 23°C, 50 mm/min | tensile yield ≥ 24 MPa |
| Thin-wall deli container | FDA 21 CFR 177.1520 | overall migration per EN 1186-1 | < 10 mg/dm² |
| Non-carbonated closure | EU 10/2011 | overall migration | < 10 mg/dm² |
| Open-top pail | UN 1H2, ASTM D1693-15 | -18°C, 10% Igepal CO-630 | no rupture; ESCR > 24 h |
| Washer reservoir | ISO 527-2, ISO 188 | 85°C, 1000 h | weld-line retention > 60% |
| Household storage | EN 71-3 | migrated elements | limit values per standard |
When Sinopec Zhenhai HDPE 7260 is used for automotive washer reservoirs, the compound is prepared at 97.0 wt% 7260 and 3.0 wt% carbon black masterbatch with 40% carbon black loading. The part is injection moulded at a melt temperature of 220°C to 240°C and a mould temperature of 15°C to 30°C. The filler neck and mounting bosses create knit lines; weld-line tensile retention is evaluated by cutting specimens parallel and perpendicular to flow from an injection-moulded plaque and testing under ISO 527-2 at 23°C and 50 mm/min. Retention below 60% of virgin yield is cause for rejection. Long-term thermal ageing is assessed under ISO 188 at 85°C for 1000 h; published data for this specific grade configuration are limited, but the resin should be restricted to washer reservoirs and exterior cold-fluid containers, not under-bonnet coolant expansion tanks exceeding 80°C or pressurised fuel-containing components. Pre-drying is required when exposure to relative humidity above 60% has occurred; a 70°C forced-air hopper dryer for 1.5 h is used before processing. Terminal parts include headlamp washer reserve tanks and windshield washer reservoirs.
Household stackable storage boxes and toy bins are moulded from 100 wt% Sinopec Zhenhai HDPE 7260 or from 98.0 wt% 7260 with 2.0 wt% colour masterbatch. Melt temperature is kept at 190°C to 220°C. The mould wall is controlled at 10°C to 20°C. Cycle time on a 350-tonne press is set by the cooling phase; reducing wall thickness below 1.5 mm requires raising melt temperature to 230°C to avoid short shots, but this increases post-mould shrinkage under ISO 294-4 above 2.0%. Colour concentrates must comply with EU 10/2011 and REACH for use in children’s articles; if the finished bin is intended for toy storage, heavy-metal release is checked under EN 71-3. Terminal parts include under-bed storage boxes, stackable toy bins, and general household utility crates.
Competitive Sinopec Zhenhai HDPE 7260 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Zhenhai HDPE 7260 is a high-density polyethylene injection moulding grade supplied by Sinopec Zhenhai Refining & Chemical Co., Ltd. It is specified for rigid packaging, thin-wall containers, crates, closures, houseware articles, and industrial inserts where medium melt fluidity, stiffness, and short cycle time are required. The grade is differentiated from blow moulding and film extrusion HDPE by its melt flow rate, molecular weight distribution, and solid-state mechanical response. Producer-published technical data for HDPE 7260 commonly report a melt mass-flow rate of 7.0 g/10 min under 2.16 kg at 190 °C measured according to GB/T 3682.1-2018 or ISO 1133-1:2022, a base density of 0.955 g/cm³ by GB/T 1033.1-2008 or ISO 1183-1:2019, and a tensile yield stress in the range 24–27 MPa when tested according to ISO 527-2:2012 at 50 mm/min. Notched Izod impact strength at 23 °C is typically reported between 3.5 and 5.5 kJ/m²; flexural modulus is usually cited between 950 and 1150 MPa under ISO 178:2019. These values are representative of commercial lots and are not specification limits; the certificate of analysis for each shipment controls final acceptance.
The principal structural difference between HDPE 7260 and high-molecular-weight blow moulding HDPE is melt viscosity. A melt mass-flow rate of 7.0 g/10 min corresponds to shorter average chain length and lower melt viscosity than a blow moulding grade in the 0.2–1.0 g/10 min range. This lower viscosity allows injection moulding of parts with flow-length-to-thickness ratios above 150:1 at moderate filling pressures, but it reduces melt strength and die swell. HDPE 7260 is therefore not intended for large-part extrusion blow moulding, corrugated pipe, or biaxially oriented film where high melt strength is needed to support the parison or bubble. Compared with a bimodal PE100 pipe grade, the grade lacks the comonomer distribution and long-term hydrostatic strength required for classification under ISO 9080.
| Parameter and test method | HDPE 7260 typical | High-molecular-weight blow moulding HDPE typical |
|---|---|---|
| Melt mass-flow rate, ISO 1133-1:2022 | 7.0 g/10 min | 0.8 g/10 min |
| Density, ISO 1183-1:2019 | 0.955 g/cm³ | 0.954 g/cm³ |
| Tensile yield stress, ISO 527-2:2012 | 25–27 MPa | 22–24 MPa |
| Flexural modulus, ISO 178:2019 | 1000–1150 MPa | 800–900 MPa |
| Notched Izod impact strength, 23 °C, ISO 180:2023 | 4.0 kJ/m² | 20 kJ/m² |
| Vicat softening temperature, ISO 306 | 125 °C | 123 °C |
The differences shown in the table are not additive by direct substitution. Replacing a high-viscosity blow moulding HDPE with HDPE 7260 in a blow moulding machine would require screw, head, and die changes to prevent draw-down and fold-backs. Conversely, using a blow moulding HDPE in an injection mould configured for HDPE 7260 would raise injection pressure and may produce short shots in thin sections.
On conventional single-screw injection moulding equipment with a general-purpose polyolefin screw of 20:1–24:1 L/D and compression ratio 2.5:1–3.0:1, HDPE 7260 is processed at melt temperatures between 190 °C and 230 °C. Mould temperatures between 15 °C and 35 °C are used for fast skin solidification. Back pressure is usually limited to 0.3–0.7 MPa, and screw surface speed is held below 0.3 m/s to limit shear heating. In thin-wall sections, flow-front velocity is typically set from 100 to 300 mm/s; above this range, jetting and flow hesitation occur at abrupt thickness changes. If the melt temperature falls below 190 °C, the first failure mode observed on the moulding line is usually flow-mark formation and weld-line cracking in ribbed sections. If the melt temperature exceeds 230 °C for more than 15 min, yellowing and odour increase, and mould deposit rates can rise.
Injection moulding lines with clamp forces from 1200 kN upward have been used to produce rigid containers and crates from HDPE 7260. Cavity-pressure transfer from filling to packing at 30–50 MPa reduces sink marks in parts with nominal wall thickness above 2.5 mm. For containers below 1.5 mm, hold pressure is commonly set between 60 and 80 MPa hydraulic unless cavity-pressure sensors are used. Thick bosses in these parts can remain molten after gate freeze; if packing time is shorter than gate-seal time, voids develop at the boss base. Gate-seal time is influenced by gate diameter and can be confirmed by cavity-pressure curve flattening rather than by machine timer alone. Shrinkage measured on plaques according to ISO 294-4:2018 is commonly 1.4–2.0% in the flow direction and 1.2–1.8% transverse. Warpage in large flat parts occurs when the differential shrinkage between flow and transverse directions exceeds 0.4 percentage points; mould cooling circuits with Reynolds number above 10,000 are used to reduce this differential.
Virgin HDPE 7260 stored in closed hoppers does not generally require predrying because polyolefin moisture uptake is below 0.01% at 50% RH. Regrind from wet granulators or outdoor silos may retain surface moisture above 0.05%, in which case drying at 80 °C for 2 h in a desiccant hopper dryer is sufficient to prevent splay. A major processing boundary is melt residence time. At 230 °C, residence should be kept below 15 min; prolonged exposure causes chain scission, surface browning, and loss of tensile yield. Lower melt temperatures reduce the risk of degradation but increase orientation and frozen-in stress in moulded parts.
When a converter removes wall thickness from 2.5 mm to 1.5 mm and uses HDPE 7260, the main processing change is the required filling pressure. Because melt flow rate is 7.0 g/10 min, the grade provides lower viscosity than an HDPE with 3.0 g/10 min, but it does not match the very high flow of 20 g/10 min thin-wall HDPE grades. At a flow-length-to-thickness ratio of 200:1, a 1.2 mm wall may require hydraulic injection pressure above 100 MPa if the melt temperature is at the lower end of the processing window. A heated sprue bushing and valve-gated hot runner with 2.0 mm gate diameter can reduce pressure loss in such geometries. Cycle-time savings are achieved mainly through faster solidification at mould temperatures of 15–20 °C, not through a large increase in melt flow.
Compared with high-flow injection HDPE grades such as 20 g/10 min HDPE, HDPE 7260 has higher flexural modulus and better ambient-temperature creep resistance, but lower notched impact strength and greater flow orientation. In closure applications with a continuous thread, hoop-stress retention after torque testing is controlled by cooling rate. Mould temperatures below 10 °C increase frozen-in stress and can cause stress cracking after contact with surfactants. Published data for environmental stress cracking resistance of this specific grade is limited; for detergent or terpene-containing products, a validated ESCR test according to ASTM D1693 or ISO 22088-2 should be performed on the moulded article.
Batch acceptance for Sinopec Zhenhai HDPE 7260 is normally performed against the producer’s certificate of analysis, which lists melt mass-flow rate, density, tensile yield stress, elongation at break, and impact strength. Because the resin is a high-density polyethylene, converters may evaluate the final article under food-contact frameworks for polyolefins such as FDA 21 CFR 177.1520 or GB 4806.6-2016; however, the resin certificate alone does not certify food-contact compliance of a moulded article. REACH and RoHS conformance are commonly declared by the producer for the resin; EU food-contact compliance must be confirmed under EU No 10/2011 using migration testing of the finished item. If the resin is used in pharmaceutical packaging, USP General Chapter 661 testing and extractables evaluation are required on the final moulding.
| Standard or regulation | Test or scope | Application relevance for HDPE 7260 |
|---|---|---|
| ISO 1133-1:2022 | Melt mass-flow rate | Injection mouldability and lot acceptance |
| ISO 1183-1:2019 | Density | Stiffness and shrinkage control |
| ISO 527-2:2012 | Tensile yield stress and elongation | Structural rigidity and ductility |
| ISO 178:2019 | Flexural modulus | Load-bearing deflection |
| ISO 180:2023 | Notched Izod impact | Drop impact and low-temperature resistance |
| FDA 21 CFR 177.1520 | Olefin polymer food-contact compositional scope | Houseware and packaging; final article testing required |
| EU No 10/2011 | Overall migration and specific migration limits | Food-contact articles sold in EU |
One production-scale limitation is the lot-to-lot variation in melt flow rate. If the MFR of a particular lot shifts from 7.0 to 6.0 g/10 min, the injection pressure may rise by 5–10% in thin-wall sections; if the MFR rises to 8.0 g/10 min, sink mark and shrinkage compensation settings may require an increase in packing pressure of 5–15%. These adjustments should be verified on the production line using cavity-pressure curves, not solely from machine hydraulic pressure.
Comparative substitution of HDPE 7260 for a general-purpose high-density polyethylene in industrial crates changes the failure mode from short-shot to sink-mark formation. On production lines producing crates with 2.8 mm nominal wall, a melt temperature of 215 °C and a mould temperature of 25 °C yield acceptable filling; however, a rib-to-wall thickness ratio above 0.7 increases sink depth beyond 0.02 mm, making the surface unacceptable for high-gloss applications. In such parts, gas-assisted injection moulding or rib redesign is required. HDPE 7260 is not used in pressure-pipe service, fuel tanks, or continuous-load creep applications where PE100 or crosslinked polyethylene classification is mandatory.