| HS Code | 209496 |
| Density | 0.954 g/cm³ |
| Melt Flow Rate | 0.9 g/10 min |
| Tensile Yield Strength | 23 MPa |
| Elongation At Break | ≥500% |
| Flexural Modulus | 1100 MPa |
| Vicat Softening Point | 125 °C |
| Brittleness Temperature | ≤ -70 °C |
| Hardness | 65 Shore D |
| Water Absorption | <0.01% |
| Environmental Stress Cracking Resistance | >1000 h |
| Dielectric Constant | 2.3 |
| Volume Resistivity | >10^16 Ω·cm |
| Thermal Conductivity | 0.44 W/m·K |
| Specific Heat | 1.9 kJ/kg·K |
| Coefficient Of Linear Thermal Expansion | 1.2×10^-4 /°C |
| Crystallinity | 85% |
| Ash Content | <0.05% |
| Moisture Content | <0.05% |
| Bulk Density | 0.55 g/cm³ |
As an accredited Sinopec Zhenhai HDPE 5000S factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinopec Zhenhai HDPE 5000S is supplied in 25 kg net PP woven bags, typically palletized at 1,000 kg per pallet. |
| Container Loading (20′ FCL) | Sinopec Zhenhai HDPE 5000S: 20′ FCL loads 25 kg bags, 1,000 bags, totaling 25 MT net weight, loose without pallets. |
| Shipping | Sinopec Zhenhai HDPE 5000S is shipped as non-hazardous high-density polyethylene resin pellets in 25 kg PP woven bags, palletized and stretch-wrapped. Typically loaded in 20' FCL containers. Store in a dry, ventilated place, away from heat, moisture, and direct sunlight. Not classified as dangerous goods. |
| Storage | Store Sinopec Zhenhai HDPE 5000S in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, and ignition sources. Keep original bags closed, palletized, and off the floor. Avoid moisture, dust, oils, and chemical contamination. Maintain stable temperature and low humidity. Protect from UV radiation, punctures, and physical damage. Use first-in, first-out stock rotation and safe stacking limits. |
| Shelf Life | Shelf life is 24 months when stored in original packaging in a cool, dry, well-ventilated area away from direct sunlight. |
Blown film lines configured with 45–65 mm grooved-feed single-screw extruders and spiral mandrel dies process HDPE 5000S at melt temperatures between 190 °C and 225 °C; the die gap is set at 0.8–1.2 mm for finished film gauges from 12 µm to 50 µm. The resin’s published melt mass-flow rate of 0.8–1.2 g/10 min under ISO 1133-1 conditions at 190 °C/2.16 kg and density of 0.953–0.956 g/cm³ under ISO 1183-1 place it in the medium-molecular-weight HDPE film class, which yields higher tensile modulus than LDPE but lower bubble stability than fractional-melt HMW-HDPE grades. Stable operation is maintained at blow-up ratios of 3.0:1 to 4.5:1, with frost-line height held at 6–10 die diameters; if the frost line drops below 5 die diameters, the film tends toward excessive orientation and loses dart impact strength measured under ASTM D1709 or ISO 7765-1. A frost line above 10 die diameters produces low machine-direction tensile strength and a wider heat-seal temperature window but reduces transverse direction tear resistance. On LDPE/LLDPE lines, HDPE 5000S is introduced at 10–30 wt% as a stiffness modifier; above 30 wt%, bubble flapping and creasing occur unless the collapsing frame angle is narrowed to 15–20° and internal bubble cooling is fitted. Barrel temperatures are profiled from 180 °C in the feed zone to 220 °C at the adapter; die head temperature is held at 210–225 °C to avoid melt fracture on the inner lip. The resultant film is used for carrier bags, bin liners, and industrial overwrap where stiffness and moisture barrier are primary requirements.
| Processing route | Melt temperature | Critical threshold | Reference standard |
|---|---|---|---|
| Blown film | 190–225 °C | Frost-line height 6–10 die diameters; blow-up ratio 3.0:1–4.5:1 | ISO 527-3, ASTM D1709 |
| Oriented tape | 190–230 °C | Draw ratio 6:1–8:1 at 100–130 °C | ISO 527-3, ASTM D4974 |
| Monofilament | 190–230 °C | Total draw ratio 7:1–9:1; finished diameter 0.20–0.40 mm | ISO 2307, ASTM D2256 |
| Sheet/thermoforming | 200–230 °C | Sheet surface 165–180 °C; chill roll 70–90 °C | ISO 178, ASTM D5748 |
| Accumulator-head blow moulding | 190–215 °C | Parison hang time 4–6 s; mould 20–30 °C | ASTM D1693, ASTM D2659 |
On industrial draw benches, HDPE 5000S tapes are extruded through slit dies of 1.6–2.5 mm width and quenched in a water bath at 30–50 °C. The quench bath temperature controls crystallite size: below 30 °C, draw tension rises and the maximum draw ratio falls; above 50 °C, width variation develops. The extruded tape thickness after quench is typically 0.04–0.06 mm. The practical draw ratio window is 6:1 to 8:1 at oven temperatures of 100–130 °C. Exceeding 8:1 without raising oven temperature above 130 °C produces fibrillation at tape edges and reduces elongation at break below 15% under ISO 527-3 or ASTM D882. Line speeds of 120–180 m/min are typical; higher speeds shorten annealing time and produce residual shrinkage above 3% under ASTM D4974. Warp tapes woven from HDPE 5000S provide sufficient tenacity for FIBC and agricultural sacks, with conditioned tenacity in the range of 0.30–0.35 N/tex under ISO 2062 or ASTM D2256. Coating with LDPE at 15–25 g/m² is required for moisture-proof applications.
With accumulator-head machines, melt temperature at the die head is controlled between 190 °C and 215 °C; above 215 °C, parison sag after 5 s hang time exceeds 15%, which restricts container size to 0.5–5 L on machines with long drop lengths. Die swell for this resin is 30–50%, so a 1 L container with an external diameter of 80 mm typically requires a die mandrel diameter near 60 mm and a die gap of 1.5–2.0 mm. Blow pressure is set at 0.6–0.8 MPa; lower pressures fail to form the pinch-off weld, while higher pressures increase flash and may cause blow-out at the weld line. Mould temperature is held at 20–30 °C; below 15 °C, the pinch-off weld becomes notch-sensitive and environmental stress cracking failures under ASTM D1693 Condition B in 10% Igepal CO-630 may occur within 20–50 h in production trials. Because published data for this specific configuration is limited, converters must run top-load strength under ASTM D2659, drop impact under ASTM D2463, and long-term creep under ASTM D2990 before qualifying containers for chemical packaging. The resin is suited to non-food containers for dilute acids, alkalis, and detergent solutions; continuous contact with aromatic hydrocarbons, chlorinated solvents, or strong oxidisers reduces ESCR and disqualifies the material unless service life is below 6 months.
Thermoformed dunnage trays and material-handling inserts are produced from HDPE 5000S sheet only when the sheet line is equipped with precise melt temperature control and the draw depth is below 150 mm; the resin’s medium molecular weight reduces hot-sag resistance compared with sheet extrusion grades below 0.5 g/10 min. On 90–120 mm extruders with flexible-lip flat dies, melt temperature is held at 200–230 °C, and chill roll temperatures are set at 70–90 °C to control crystallinity and surface finish. The die gap is maintained at 1.5–2.0 times the finished sheet gauge, typically 1.2–3.0 mm for dunnage applications. In the thermoformer, sheet surface temperature must remain between 165 °C and 180 °C as measured by infrared pyrometer; the grade’s crystalline melting peak lies near 130–135 °C by differential scanning calorimetry. Above 180 °C, the sheet sags into the lower heater bank and produces non-uniform wall thickness; below 165 °C, plug penetration generates stress whitening and lowers flexural modulus under ISO 178 or ASTM D790. Plug-assist forming with aluminium plugs maintained at 90–110 °C and plug speeds of 200–400 mm/s is used for shallow trays. Finished trays are evaluated for puncture resistance under ASTM D5748 and low-temperature drop impact under ASTM D2463. Trim regrind is incorporated at 20–40 wt% after screening through a 40 mesh screen pack; higher regrind levels reduce melt temperature consistency and increase gel particle counts in the finished sheet.
At line speeds above 120 m/min, monofilament extrusion of HDPE 5000S loses diameter control unless the gear pump pressure fluctuation is below 0.2 MPa. A 45–65 mm single-screw extruder feeds a strand die with 24–48 holes of 0.5–1.2 mm diameter; the melt temperature at the die is 190–230 °C. The extrudate is quenched in a water bath at 35–55 °C, then drawn through a first-stage oven at 90–110 °C and a second-stage oven at 110–125 °C. The total draw ratio is held at 7:1 to 9:1 for finished filament diameters of 0.20–0.40 mm. Above 9:1, the filament surface becomes fibrillated and the elongation at break falls below 20%, reducing knot strength under ISO 2307. Finished filaments are used in shade netting, anti-hail nets, and braided rope cores; outdoor service beyond 2–3 years requires carbon black masterbatch at 2.0–2.5 wt% or hindered amine light stabilisers at 0.1–0.3 wt% to pass accelerated weathering under ISO 4892-2 or ASTM G154. Tensile properties are measured under ISO 2062 or ASTM D2256, and mesh strength of finished nets under ISO 1805. Published data for this specific configuration is limited; production trials must therefore establish the exact draw ratio by tensile testing across the first 24 h of continuous output.
The environmental stress cracking resistance of HDPE 5000S governs its use in rigid packaging for aggressive chemical formulations. Under ASTM D1693 Condition B in 10% Igepal CO-630 at 50 °C, the grade is expected to exceed 100 h without failure when moulded at 20–30 °C; lower mould temperatures and sharp weld-line notches reduce the time to failure to 20–50 h in some production trials. For household and industrial chemical packaging, the resin is compatible with dilute acids, alkalis, and detergent solutions; continuous exposure to aromatic hydrocarbons, chlorinated solvents, and strong oxidizers reduces ESCR and requires replacement with a higher-MFR or crosslinked HDPE grade if service life exceeds 6 months. The density of 0.953–0.956 g/cm³ yields lower water vapour transmission than LLDPE film grades, but oxygen barrier remains insufficient for oxygen-sensitive products without a barrier layer. Food-contact applications require converter verification under FDA 21 CFR 177.1520(c) for olefin polymers, including extractives limits for the intended food type and use condition; for EU markets, overall migration testing under Regulation (EU) No 10/2011 and specific migration limits for additives must be completed on the finished article. REACH compliance is typically based on the supplier’s registration dossier for the polymer; industrial users must verify that recycled content or processing aids added during conversion do not introduce SVHCs above 0.1 wt%. End-use testing commonly includes total migration under EN 1186, packaging heavy metals under 94/62/EC, and specific migration of antioxidants under EU 10/2011 Annex V.
Competitive Sinopec Zhenhai HDPE 5000S prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Zhenhai HDPE 5000S is a high-density polyethylene extrusion resin supplied in 25 kg bags. It is specified for high-tenacity monofilament, stretched tape, rope and woven-sack tape because its nominal melt mass-flow rate of 0.9 g/10 min at 190 °C under 2.16 kg load, measured to ISO 1133-1, provides sufficient melt strength during free-surface drawing. The pellet density is 0.954 g/cm3 at 23 °C per ISO 1183-1. In low-MFR HDPE conversion, the combination of low melt flow and high crystallinity permits stable neck formation in water-quench tape lines; it is not a thin-wall injection-moulding grade. Production-scale use is concentrated in lines equipped with 65–90 mm grooved-feed single-screw extruders and L/D 30:1 or 33:1 screws. The following table lists representative property values from producer technical data; multi-lot ranges may vary and should be verified against the certificate of analysis.
| Property | Test method | Representative value |
| Melt mass-flow rate, 190 °C/2.16 kg | ISO 1133-1 | 0.8–1.2 g/10 min |
| Density, 23 °C | ISO 1183-1 | 0.953–0.956 g/cm3 |
| Tensile stress at yield, 50 mm/min | ISO 527-2 | 23–26 MPa |
| Tensile elongation at break | ISO 527-2 | >600% |
| Notched Charpy impact strength, 23 °C | ISO 179-1/1eA | 15–25 kJ/m2 |
| Vicat softening temperature, A50, 10 N | ISO 306 | 123–127 °C |
| Shore D hardness | ISO 868 | 61–65 |
At nominal 0.9 g/10 min MFR, the melt exhibits high viscosity relative to injection HDPE grades with MFR above 5 g/10 min. In 90 mm grooved-feed extruders operating at 250–300 kg/h, die head pressure is typically recorded between 18 MPa and 26 MPa when melt temperature is controlled at 210–225 °C. The high-molecular-weight fraction raises elongational viscosity during drawing, but it also increases screw motor load. A screw with L/D 30:1, a barrier section and a Maddock or pin mixing section reduces melt-temperature non-uniformity compared with a three-zone screw. Pressure at the breaker plate above 28 MPa at constant throughput is a production-scale indicator of screen-pack fouling from oxidised polyethylene gel or foreign matter; it should not be interpreted as an increase in resin intrinsic viscosity. Converter records indicate that melt-temperature overshoot above 230 °C accelerates gel formation and raises die-lip deposit frequency on flat dies. The product does not exhibit strain-hardening behaviour typical of branched low-density polyethylene under film blowing; published extensional viscosity data for 5000S is limited.
Flat-die tape lines typically use a die gap of 0.8–1.2 mm and a land length of 10–15 times the gap. Monofilament spinnerets use holes from 0.6 mm to 1.0 mm; hole-to-hole pressure variation is kept below 0.3 MPa by melt-pump control. The die lips are chromed or otherwise coated to reduce exudate accumulation. A screen pack of 40/60/120 mesh is common, but converter trials with 150 mesh reduce gel breaks at the cost of increased pressure. Because 5000S has low MFR, finer filtration raises head pressure quickly; a new 150 mesh pack can add 2–4 MPa pressure rise compared with 120 mesh at 250 kg/h. Melt temperatures above 220 °C increase oxidised gel formation at the die lip, particularly during line stops longer than 15 min. Start-up after a stop should include purging with neat HDPE until die pressure stabilises below 26 MPa.
In water-quench monofilament and tape lines, the melt exits a flat die or spinneret into a water bath maintained at 20–35 °C. The water-air gap is normally held between 15 mm and 40 mm to limit die-face cooling while avoiding excessive air drag. Quench cooling fixes the primary crystallinity and creates a fine spherulitic structure that can be drawn to high orientation. The low MFR of 5000S stabilises the neck under draw ratios of 8:1 to 10:1; at these ratios and 0.8–1.2 mm die gaps, final tape widths remain within ±3% on lines with melt pumps. Orientation is performed on heated godets or in hot-air ovens at 90–100 °C. Isotropic tensile values from ISO 527-2 compression-moulded plaques do not predict oriented tape tenacity; oriented tape properties are governed by draw ratio, quench temperature, die gap and molecular-weight distribution. Converter specifications for oriented tenacity must be negotiated on a line-specific basis because the producer data sheet does not assign a universal tenacity value.
The primary process boundaries are draw resonance, fibrillation and gel-related break. Draw resonance appears as periodic diameter variation when the draw ratio exceeds the strain-hardening capacity of the melt. In 5000S, stable drawing is maintained at 8:1 to 10:1 with quench water at 25 ± 3 °C and a draw gap of 15–40 mm. At draw ratios above 12:1, filament breaks correlate with quench-bath turbulence and godet speed oscillations rather than melt fracture at the die. Because the grade has a broad molecular-weight distribution, it is less prone to narrow-window draw resonance than metallocene LLDPE, but it requires more consistent quench temperature. Gel particles above 200 µm originating from oxidised resin, screen-pack degradation or cross-contamination with incompatible polymers act as stress concentrators during solid-state drawing and cause filament snap at the water line. Pressurised melt pumps reduce die-inlet pressure fluctuation to below 0.5 MPa; higher fluctuation changes tape width uniformity by more than 2% in 0.8 mm die-gap lines. These threshold values come from converter operation on comparable low-MFR HDPE monofilament lines; published data for this specific configuration is limited.
Differentiation is made primarily through flow, density and orientation stability. The table below compares 5000S with a medium-flow injection-moulding HDPE and a high-melt-strength blow-moulding HDPE. Product names are omitted where exact portfolio designations are not public.
| Characteristic | 5000S | Typical injection HDPE | Typical blow-moulding HDPE |
| MFR, 190 °C/2.16 kg | 0.9 g/10 min | 6.0 g/10 min | 0.35 g/10 min |
| Density, 23 °C | 0.954 g/cm3 | 0.956 g/cm3 | 0.948 g/cm3 |
| Tensile stress at yield | 23–26 MPa | 25–28 MPa | 21–24 MPa |
| Primary conversion route | tape or monofilament extrusion | injection moulding | blow moulding |
| Melt strength under free-surface drawing | high | low | very high |
| Draw ratio stability in water-quench tape | stable at 8:1–10:1 | unstable at 8:1 | stable but high extruder load |
The 0.9 g/10 min MFR of 5000S supports free-surface drawing in tape and monofilament lines. A 6.0 g/10 min injection grade fills thin-wall moulds at lower melt pressure and faster screw recovery but lacks the melt strength required to maintain a stable neck at 8:1 draw; the same draw ratio produced periodic diameter fluctuation in comparative converter trials. A 0.35 g/10 min blow-moulding grade delivers higher melt strength but increases extruder motor load and often requires higher barrel temperatures to reach equivalent throughput. The density difference of 0.948–0.956 g/cm3 across these grades also shifts crystallinity and final part stiffness; 5000S is therefore neither a general-purpose injection grade nor a high-melt-strength blow grade. Its additive package is chosen for low die-lip deposit in orientation lines; converters moving a blow-moulding grade into tape production should verify gel count and screen-pack pressure rise.
Because low-MFR HDPE grades from alternate licensors can differ in molecular-weight distribution, gel count and additive package, substitution on MFR and density alone is not sufficient. Two resins both carrying 0.9 g/10 min MFR and 0.954 g/cm3 density may differ in comonomer type, catalyst residue and long-chain branching. In high-tensile tape drawing, batch-to-batch differences in these variables shift the maximum stable draw ratio by 1–2 units and alter water-quench sensitivity. The producer certificate of analysis should therefore include MFR, density, tensile yield, elongation and notched Charpy impact as minimum data. Gel count and screen-pack pressure rise are not always disclosed; converters should request a processing trial when changing supplier. Published data for this specific configuration is limited.
Storage below 50 °C and protection from direct UV radiation reduce oxidative surface degradation. HDPE 5000S does not require routine pre-drying, but pellets stored where ambient relative humidity exceeds 80% RH can carry surface moisture that forms steam bubbles at the die lip during tape extrusion. Pre-drying at 60 ± 5 °C for 2 h in hot-air or desiccant hopper dryers is sufficient for such conditions. The product is not to be blended with polypropylene, nylon or PET unless a dedicated compatibilised formulation has been validated; these polymers separate in the melt and create delamination sites in drawn tape. Food-contact suitability is not automatically conferred by the base resin; converters must verify FDA 21 CFR 177.1520 or EU Regulation 10/2011 compliance for the final article, including specific migration limits and the actual additive package. REACH and RoHS status is batch-dependent and should be confirmed against the safety data sheet and supplier certification. No process guarantee applies outside the documented operating window of 200–220 °C melt temperature and draw ratios below 12:1.