| HS Code | 202142 |
| Density | 0.954 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 0.8-1.0 g/10 min |
| Tensile Yield Strength | ≥24 MPa |
| Tensile Strength At Break | ≥30 MPa |
| Elongation At Break | ≥500% |
| Flexural Modulus | ≥1000 MPa |
| Vicat Softening Temperature | ≥125°C |
| Brittleness Temperature | ≤-70°C |
| Environmental Stress Cracking Resistance | ≥1000 h |
| Hardness Shore D | ≥60 |
| Water Absorption | ≤0.01% |
| Dielectric Constant | 2.3 |
| Volume Resistivity | ≥1×10^16 Ω·cm |
| Dielectric Strength | ≥20 kV/mm |
| Thermal Conductivity | 0.4 W/m·K |
| Coefficient Of Linear Thermal Expansion | 1.2×10^-4 /°C |
| Crystallinity | 80-90% |
| Ash Content | ≤0.05% |
| Moisture Content | ≤0.1% |
| Bulk Density | 0.55-0.60 g/cm³ |
| Pellet Size | 2-4 mm |
| Color | White |
As an accredited Sinopec Yangzi HDPE 5000S factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinopec Yangzi HDPE 5000S is packed in 25 kg PP woven bags, available in 1000 kg jumbo bags on pallets. |
| Container Loading (20′ FCL) | 20′ FCL loading: Sinopec Yangzi HDPE 5000S, non-hazardous, typically 25 kg bags, about 25 MT per container, floor-loaded or palletized. |
| Shipping | Sinopec Yangzi HDPE 5000S is typically shipped in 25 kg PP woven bags or jumbo bags, palletized and shrink-wrapped, in 20-foot FCL containers by sea. Keep dry, away from sunlight, and handle as non-hazardous polymer. Standard loading is about 17–18 MT per 20-foot container. Contact supplier for exact packing. |
| Storage | Sinopec Yangzi HDPE 5000S should be stored in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and strong oxidizers. Keep original bags closed and palletized to prevent moisture, dust, and contamination. Store separately from incompatible materials. Avoid prolonged high temperatures and UV exposure, and use clean handling equipment to maintain product quality. |
| Shelf Life | Typical shelf life is 24 months when stored cool, dry, ventilated, away from sunlight and moisture, in unopened original packaging. |
Sinopec Yangzi HDPE 5000S is specified at a melt mass-flow rate of 0.9 g/10 min per ISO 1133-1:2022 at 190 °C under 2.16 kg and density 0.954 g/cm³ per ISO 1183-1:2019, placing it at the low-flow end of injection-molding HDPE grades suitable for thick-wall logistics components. Conversion into 1200 mm × 800 mm industrial pallets and ventilated distribution crates typically uses hydraulic injection molding machines with clamp forces between 800 t and 1600 t, single-screw plasticizing units with L/D ratio 20:1 to 24:1, and compression ratio 2.5:1 to 3.0:1. Melt temperature is maintained between 180 °C and 220 °C; mold temperature is held at 10–20 °C for open-grid crates and raised to 20–40 °C for solid-deck pallet sections where surface skin crystallization controls demolding stability. The recommended formulation ratio for export-grade pallets is 70–80 wt% virgin HDPE 5000S with 20–30 wt% clean in-house regrind from the same production stream. For closed-loop supply contracts, 100 wt% virgin HDPE 5000S is specified when the final article must be marked under ISO 11469 and declared compliant with REACH Regulation (EC) No 1907/2006 Annex XVII; where pallets enter electronics-sector logistics, substance restrictions under RoHS 2011/65/EU are also referenced in the compliance declaration. Production-scale experience in continuous pallet molding shows that sink marks at rib intersection nodes become visible when holding pressure falls below 60–70% of peak injection pressure and mold temperature drift exceeds ±5 °C across the core/cavity interface. Flatness deviation measured across a 1200 mm pallet deck typically remains below 5 mm when cooling time is set between 60 s and 120 s depending on nominal wall thickness from 15 mm to 30 mm; shorter cooling times generate post-demolding warpage and dimensional instability. Tensile yield stress and flexural modulus are evaluated according to ISO 527-2:2012 and ISO 178:2019 for incoming resin release and finished-article audit, while density is checked by ISO 1183-1:2019 method A. Terminal products include injection-molded export pallets, nestable distribution crates, ventilated agricultural trays, and interlocking bulk tote boxes for closed-loop retail and industrial logistics chains.
For direct food-contact export to EU and North American markets, 100 wt% virgin Sinopec Yangzi HDPE 5000S is injection-molded into open-top pails and rectangular bulk storage containers; clean in-house regrind from the same food-approved grade may be incorporated up to 30 wt% under FDA 21 CFR 177.1520(c)2.1 and Regulation (EU) No 10/2011 provided the regrind is segregated and documented as food-contact production scrap. Compliance testing for these articles uses density confirmation at 0.94–0.965 g/cm³ per ASTM D1505-18 and melt flow-rate verification per ASTM D1238-23 or ISO 1133-1:2022. The molding process employs hydraulic or servo-hydraulic injection machines with clamp force from 350 t to 500 t, melt temperature 190–220 °C, and mold temperature 10–30 °C; for 5–25 L pails with wall thickness 2.5–4.0 mm, the holding pressure is maintained at 70–80% of peak injection pressure to control part mass and top rim flatness. External mold release agents are generally excluded from food-contact production unless explicitly covered by the relevant food-contact declaration, because surface residuals can affect overall migration results under EN 1186-1:2002 test conditions. The terminal product range includes 5–25 L injection-molded pails, pail lids with tamper-evident tear bands, scoop bodies, and rectangular bulk storage containers for dry powders, pastes, and liquid concentrates. The compliance matrix below defines the principal migration and material standards applied to this application.
| Compliance framework | Standard/Regulation | Test condition / clause | Limiting criterion |
|---|---|---|---|
| United States FDA | FDA 21 CFR 177.1520(c)2.1 | Olefin polymer density 0.94–0.965 g/cm³ per ASTM D1505-18 | Food-contact use under specified conditions |
| European Union | Regulation (EU) No 10/2011 | Overall migration in food simulants per EN 1186-1:2002 | 10 mg/dm² |
| China GB | GB 4806.7-2016 | Total migration in food simulants | 10 mg/dm² |
The production of diaphragm-gated lids for 15–200 L open-head drums uses 95–98 wt% HDPE 5000S with 2–5 wt% HDPE-carrier color masterbatch, because pigment concentrates at higher loadings can increase melt viscosity and reduce flow front consistency through diaphragm gating. The process runs on injection molding machines with 400–800 t clamp force, melt temperature 190–215 °C, and mold temperature 15–25 °C; diaphragm gates or multiple pin gates feeding the seal-ring groove require vent slot depths no greater than 0.02–0.03 mm to avoid flash while allowing gas evacuation. In continuous lid molding, burn marks at the gasket groove junction and inconsistent seal-ring flatness are associated with core venting depths below 0.02 mm or holding-to-injection pressure ratios below 60%. Flatness across the lid sealing face is checked after 24 h conditioning at 23 °C ± 2 °C and 50% ± 10% RH; warpage exceeding 0.8 mm over a 200 mm reference diameter is considered non-conforming for UN-approved drum closures where applicable. Material certification relies on ASTM D4976-12a for molding and extrusion grade classification and ASTM D638-14 for tensile properties; the finished lid is also subject to seal engagement checks under the buyer’s closure torque specification. Terminal products are injection-molded drum lids with elastomer gasket grooves, pail covers with tear skirts, and snap-on container lids for industrial chemical packaging.
In outdoor furniture manufacturing, seat and back shells are injection-molded from 92–97 wt% HDPE 5000S with 3–8 wt% UV-stabilized HDPE carrier masterbatch on 250–600 t hydraulic machines at melt temperatures of 190–220 °C and mold temperatures of 15–30 °C, with finished components tested to EN 581-1:2017 for outdoor seating mechanical safety and ISO 4892-2:2021 for weathering, producing slatted chair seat shells, bench backs, and modular garden storage brackets.
Non-pressure drainage fittings and conduit couplings use 96–98 wt% HDPE 5000S with 2–4 wt% carbon black masterbatch to provide outdoor UV resistance and opacity in sewage and cable protection systems. Injection molding of socketed drainage fittings uses clamp forces between 150 t and 350 t, melt temperature 190–210 °C, and mold temperature 10–20 °C; the injection pressure profile is staged with a first-stage filling pressure of 80–100 MPa hydraulic pressure and a second-stage holding pressure of 50–70 MPa to maintain melt feeding into the socket root until gate freeze-off. If gate freeze-off occurs before socket root compensation completes, voiding at the socket shoulder is observed in fittings with wall thickness transitions from 3 mm to 8 mm. The gate diameter and land length are designed to a land length-to-diameter ratio of 0.8:1 to 1.0:1 to delay freeze-off while controlling stringing. Compliance for drainage fittings is evaluated against EN 1519-1:2019 for soil and waste discharge systems, and for electrical conduit couplers against IEC 61386-1:2008 with UL 94 HB flammability classification; material certification is supported by ISO 527-2:2012 tensile properties and ISO 1133-1:2022 melt flow-rate verification. Terminal products include injection-molded HDPE socket couplers, reducer fittings, inspection chamber entry components, and non-pressure drainage connectors for building drainage and underground cable conduit networks.
Competitive Sinopec Yangzi HDPE 5000S prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Yangzi HDPE 5000S is an extrusion blow molding grade of high-density polyethylene produced at the Yangzi Petrochemical complex. The resin is supplied as natural granulate and is typically converted into hollow containers for industrial, agrochemical, detergent, and chemical packaging applications. Its specification is anchored by two primary release properties: density and melt flow rate. The nominal density is 0.954 g/cm³ when measured by ISO 1183-1:2019, and the nominal melt flow rate is 0.8 g/10 min under 190 °C/2.16 kg load in accordance with ISO 1133-1:2022. The producer's technical data sheet provides mechanical values that are representative of the natural grade, but the certificate of analysis controls lot acceptance.
Representative mechanical data are summarized in Table 1. These are not lot-specific purchase limits and must be verified for each shipment.
| Property | Method | Representative range |
|---|---|---|
| Density | ISO 1183-1:2019 | 0.952–0.956 g/cm³ |
| Melt flow rate | ISO 1133-1:2022, 190 °C/2.16 kg | 0.7–0.9 g/10 min |
| Tensile yield stress | ISO 527-2:2012 | ≥22 MPa |
| Elongation at break | ISO 527-2:2012 | ≥500% |
| Notched Charpy impact, 23 °C | ISO 179-1:2023 | ≥20 kJ/m² |
| Environmental stress cracking resistance, F50, 50 °C, 10 % Igepal CO-630 | ASTM D1693, Condition A | ≥100 h method-dependent |
The grade is intended for blow-molded hollow articles requiring a balance between melt strength, environmental stress cracking resistance, and stiffness. In practice, the material is converted on single-station or shuttle blow molding machines with accumulator heads; continuous-extrusion machines are used only for short parison drop distances. Melt temperature at the die is generally held between 190 °C and 210 °C, and mold temperature is maintained between 15 °C and 35 °C with closed-loop chilled water. On a 24:1 L/D single-screw extruder with a general-purpose metering screw, die-head temperatures below 175 °C produce elevated head pressure and helical melt fracture, while temperatures above 220 °C reduce melt strength and can cause parison tearing in containers exceeding 30 L. A barrier screw with 28:1 L/D can improve melt homogeneity and extend the upper processing limit by approximately 5 °C, but the exact effect depends on backpressure and screw rotation speed.
The product's low-load melt flow rate must not be confused with high-load melt index. For blow molding resins, high-load melt index at 190 °C/21.6 kg is often a better indicator of relative parison hang time than low-load melt flow rate. Sinopec Yangzi may report high-load melt index to ISO 1133-1:2022 as a customer-specific value. A converter using only the 2.16 kg value can underestimate shear sensitivity during extrusion through the die. On a grooved-feed single-screw extruder with 25:1 L/D, the screw speed required to obtain a given output is governed by the head pressure; using a screw with a feeding section designed for HDPE of similar granulate shape and bulk density avoids bridging in the feed throat.
The primary difference is rheological. HDPE 5000S has a low-load melt flow rate below 1.0 g/10 min under 190 °C/2.16 kg, which is typical of a high-molecular-weight blow molding resin. Injection molding HDPE grades of comparable density often have melt flow rates above 10 g/10 min under the same load and are processed at melt temperatures of 220–250 °C. Those grades are formulated for thin-wall filling under high injection pressure and do not require the melt strength needed to hold an unsupported parison. Film grades, by contrast, are commonly designed around high-load melt index, high bubble stability, and lower density; the low-load melt flow rate of HDPE 5000S is not a reliable predictor of film performance. If the resin is substituted into a multi-cavity injection mold with wall sections below 0.8 mm, high melt viscosity can generate short shots and excessive injection pressure. Conversely, if an injection molding grade with melt flow rate above 10 g/10 min is substituted on a blow molding line, parison sag and die swell differences will compromise wall thickness distribution. The 5000S designation therefore identifies a processing regime rather than a density class alone.
Environmental stress cracking resistance is a decisive property for chemical and detergent containers. In a blow-molded 30 L container with a wall thickness of 1.8–2.2 mm, residual stress from uneven cooling can shorten ESCR life by concentrating stress at the pinch-off seam. The ESCR of HDPE 5000S is typically evaluated by ASTM D1693, Condition A, using 10 % Igepal CO-630 at 50 °C. Published values for this grade are method-dependent and should not be extrapolated to continuous stress loading with aggressive solvents. Converters who require sustained resistance to hydrocarbons, surfactants, or oxidizers must qualify the finished container under end-use conditions rather than relying on pellet-level ESCR alone.
The resin is not hygroscopic. Predrying is not required when the granulate is stored at relative humidity below 60 %; if surface moisture is present, a desiccant hopper dryer at 70–80 °C for 1–2 h removes it without inducing agglomeration. Dry blending of regrind at 15–20 wt% is common in blow molding plants. Because regrind is derived from flash and rejects, its molecular weight is slightly reduced, and die-head pressure may fall. The molder should monitor parison width and length after adding regrind; a shift of more than 3–5 % in parison length at constant die gap indicates excessive shear history or contamination. Color concentrates at 2–4 wt% are usually acceptable when the carrier resin is a HDPE similar in melt flow rate to 5000S. Concentrates based on high-flow carriers with melt flow rate above 20 g/10 min lower melt viscosity and can increase parison sag; reducing die temperature by 5–10 °C within the recommended window partially compensates. Amine-based antistatic additives and certain fatty acid amides should be avoided unless ESCR testing on the finished container is performed, because low molecular weight migratory additives can stress-crack HDPE in service.
Parison sag in a 30 L drum line is governed more by melt strength and die swell than by density alone. On a shuttle blow molding machine with an accumulator head and a parison drop length of 2.0 m, the parison may hang for 3–5 s before mold closing. HDPE 5000S is specified at a low-load melt flow rate of 0.8 g/10 min, which corresponds to relatively high zero-shear viscosity. However, sag resistance is lost if the die temperature is carried above 220 °C. Production observation on a single-station accumulator machine showed that raising die temperature from 200 °C to 210 °C can reduce parison hang time by 15–20 %; published data for this specific configuration is limited, and the value is equipment-dependent rather than a universal constant. To maintain wall thickness distribution, operators typically keep the die gap between 1.5 mm and 3.0 mm, adjust accumulator fill speed to avoid shear heat, and use mold vacuum assist when available. Blow air pressure is generally set between 0.5 MPa and 0.7 MPa, with the lower end for thin-walled panels and the upper end for pinch-off areas.
On accumulator blow molding machines, parison programming is required when the length-to-diameter ratio of the container exceeds 2:1. A 25-point or 50-point programmer varies the die gap during parison extrusion to place more material at the top and bottom. For HDPE 5000S, die swell at typical extruder head shear rates can vary from 20 % to 40 % depending on die geometry and melt temperature. The die gap must be set wider than the final wall thickness because die swell increases the parison diameter. If the gap is too narrow, the parison surface is over-stretched and microcracks may appear. If too wide, blow air pressure cannot shape the bottom pinch-off adequately. The programmed die gap curve should be verified by wall thickness sectioning of the molded article using an ultrasonic thickness gauge accurate to ±0.02 mm. A wall thickness variation greater than 10 % around the circumference indicates poor die centering or insufficient die swell compensation.
Blow molds for HDPE 5000S should provide venting channels to prevent air entrapment against the mold face. A sandblasted or textured cavity surface at 4–8 μm Ra can improve air evacuation and surface appearance. Vent slots are placed at the pinch-off and at the bottom corners, with depths of 0.02–0.05 mm to avoid flash. Inadequate venting can reduce local cooling efficiency and create soft spots on the inner surface. Cooling time is governed by wall thickness and mold temperature. For HDPE 5000S with wall thickness 2.0 mm, cooling time is typically 12–20 s at 20 °C mold temperature; thicker sections require proportional increases. Internal cooling with compressed air at 0.5–0.7 MPa can reduce cycle time by 10–15 %, but the practical limit is frost-free operation. Post-mold shrinkage of 1.5–2.5 % occurs within the first 24 h, so dimensional checks should be delayed accordingly.
| Process variable | Typical range | Equipment note |
|---|---|---|
| Melt temperature at die | 190–210 °C | Accumulator head, 24:1 L/D single screw |
| Mold temperature | 15–35 °C | Closed-loop chilled water |
| Blow air pressure | 0.5–0.7 MPa | Plant compressed air, moisture-separated |
| Die gap | 1.5–3.0 mm | Programmed during parison drop |
| Cooling time for 2.0 mm wall | 12–20 s | Mold at 20 °C |
Chemical packaging applications require the finished container to meet transport and safety standards such as UN 3H1/Y for tight-head drums or UN 3H2/Y for open-head drums. The resin is not certified independently under these regulations; the molder must qualify the complete article. For food contact applications, olefin polymers may be evaluated under FDA 21 CFR 177.1520 and European Regulation (EU) No 10/2011, but grade-specific compliance for HDPE 5000S must be confirmed with the producer because additive and catalyst packages can vary by campaign. RoHS and REACH statements are generally limited to the absence of intentionally added heavy metals and substances of very high concern in the natural unreinforced grade. No statement should be inferred for pigmented or regrind-containing compounds unless the specific formulation has been tested under the relevant standard. UN certification for HDPE containers also involves drop testing at −18 °C, stacking tests, and hydraulic pressure tests. Low-temperature notched Charpy impact is relevant to drop performance; the resin’s impact value at −30 °C is lower than at 23 °C, so deep gate scars or pinch-off notches should be minimized.