| HS Code | 506355 |
| Density | 0.954 g/cm³ |
| Melt Flow Rate Mfr 190 C 2 16 Kg | 0.35 g/10 min |
| Melting Point | 133 °C |
| Vicat Softening Point | 125 °C |
| Tensile Strength At Yield | ≥25 MPa |
| Elongation At Break | ≥600% |
| Flexural Modulus | ≥1100 MPa |
| Notched Izod Impact Strength | ≥50 kJ/m² |
| Environmental Stress Cracking Resistance Escr | ≥1000 h |
| Brittleness Temperature | ≤ -70 °C |
| Shore D Hardness | ≥60 |
| Water Absorption | ≤0.01% |
| Ash Content | ≤0.05% |
| Volatile Matter | ≤0.1% |
| Crystallinity | ≥70% |
As an accredited Sinopec Wuhan HDPE HD5502W factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinopec Wuhan HDPE HD5502W is packed in 25 kg woven bags, palletized, and stretch-wrapped, with 1,000 kg per pallet. |
| Container Loading (20′ FCL) | Sinopec Wuhan HDPE HD5502W: 25kg bags; 20′ FCL loads approximately 17–18 MT net, palletized or loose, depending on packing requirements. |
| Shipping | Sinopec Wuhan HDPE HD5502W is a non-hazardous high-density polyethylene resin. It is typically shipped in 25 kg woven bags or 500–1000 kg jumbo bags, palletized and stretch-wrapped, via dry containers or trucks. Keep dry, away from heat and direct sunlight. Standard shipping documents apply; no special dangerous goods handling required. |
| Storage | Store Sinopec Wuhan HDPE HD5502W in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and strong oxidizers. Keep original packaging sealed, palletized, and off the floor. Avoid moisture, dust, and contamination. Do not stack excessively high to prevent bag deformation. Maintain good housekeeping, follow local regulations, and use first-in, first-out inventory. |
| Shelf Life | Shelf life: 24 months when stored in original packaging in a cool, dry, well-ventilated place, away from direct sunlight and moisture. |
In the agrochemical packaging sector, HD5502W is processed as the main wall material for UN-certified jerrycans filled with glyphosate, acetochlor and abamectin formulations. The grade is a unimodal blow-molding HDPE with a density of 0.955 g/cm³ (ISO 1183-1:2019) and a melt-flow rate of 0.35 g/(10 min) (ISO 1133-1:2022), placing it in the high-melt-strength class required for a 25-L tight-head jerrican with a minimum sidewall of 0.9 mm. Production-scale trials on a single-station shuttle blow molder with an 80-mm grooved-feed extruder (L/D 30:1) and an accumulator head of 1.5-kg shot size establish a feed-to-die profile of 180/190/195/200°C; the head temperature is held at 202–208°C. The compound is 100 phr HD5502W, 2.5 ± 0.5 wt% carbon black masterbatch (40% pigment in an LLDPE carrier), 0.1–0.2 wt% hindered phenolic-phosphite antioxidant masterbatch, and ≤20 wt% post-industrial regrind. Regrind above 30 wt% reduces the ESCR below 250 h under ASTM D1693-15 condition B in xylene-based test liquids. A mold temperature of 15–25°C and a blow pressure of 0.6–0.8 MPa are used. Wall thickness is measured by ultrasonic gauge after cooling; typical pinch-seam readings are 1.4 mm, and the chimb is 0.9 mm. Post-consumer material is not introduced because residual silicone mold-release agents and amine-based antistatic compounds from detergent bottle streams can accelerate stress cracking. Compliance is anchored to UN Model Regulations Chapter 6.1 for Packing Group II, 49 CFR §178.512, and ADR 6.1.4. Finished articles include 20-L, 25-L and 30-L tight-head jerricans with UN 3H1 or UN 3H2 marking, 5-L calibrated dosing bottles, and pour-spout closures with EPE liners.
| Test | Method/standard | Packing Group II condition | Monitored wall variable |
|---|---|---|---|
| Free-fall drop | UN 6.1.4.2 | 1.2 m at 20°C; relative density ≤1.2 | Pinch seam integrity, sidewall cracking |
| Hydraulic pressure | UN 6.1.4.6 | 100 kPa for 30 min | Dome deformation, weld line leakage |
| Stacking | UN 6.1.4.8 | 40°C for 28 days | Top-load buckling, closure retention |
Continuous shuttle blow molding of 5-L narrow-mouth lubricant bottles exposes HD5502W to high shear at the die lip and rapid cooling against a 10°C mold surface. The bottle must tolerate motor-oil fill at 40°C and stack loads of 8–10 cartons in warehouse storage. The compound is 100 phr HD5502W, 2.0–3.0 wt% white masterbatch (60% TiO₂ in LDPE), 0.15 wt% calcium stearate, and 0.05 wt% fluoropolymer processing aid; the processing aid is introduced only when surface die lines exceed 2.0 mm length on the bottle shoulder. Internal regrind from bottle tails is added at 15–25 wt% after granulate homogenization. Melt temperature is maintained at 208–215°C. Below 202°C the parison surface exhibits melt fracture at the handle bridge, and above 218°C the sidewall thickness at the bridge drops below 0.6 mm. The machine is a 70-mm extruder with L/D 25:1 and an 8-cavity shuttle mold. Blow pressure is 0.6–0.7 MPa. Compliance for nonhazardous lubricant bottles does not require UN marking; however, when the lubricant is classified under UN 6.1 as Packing Group III, the bottle is qualified at a drop height of 0.8 m, and closure torque retention is tested at −20°C. Marking follows ISO 780:2015. Article types are 1-L, 4-L and 5-L standard and extended-nap bottles for SAE 15W-40 engine oil, ISO VG 46 hydraulic oil, and high-detergent diesel crankcase blends.
Diesel exhaust fluid (DEF) tanks manufactured from HD5502W are subjected to a 32.5 wt% aqueous urea solution that freezes at −11.5°C and expands by approximately 7% in volume at the solidification point. The critical failure site is not the tank shell but the 90° fill neck and the molded-in bracket boss; stress cracks initiate there after repeated freeze-thaw cycling. Processing on a 100-mm accumulator-head blow molder with L/D 30:1 extruder uses a melt temperature of 210–220°C, a blow pressure of 0.7–0.9 MPa, and a mold temperature of 15–20°C. The additive formula is 100 phr HD5502W, 2.5 wt% carbon black masterbatch, 0.3 wt% HALS-based UV stabilizer, 0.1 wt% hindered phenolic antioxidant, and 0.2 wt% fluoropolymer processing aid. Regrind is capped at 30 wt% and pre-dried at 80°C for 4 h when silo RH exceeds 60%. The temperature window at the accumulator head is limited to ±3°C because parison weight varies by 6–8% outside 205–220°C, creating thin spots at the fill neck and the baffle plate. The tank shell is programmed to 3.0–4.0 mm at the lower chimb and 2.5 mm at the sidewall. Compliance rests on ISO 22241-3:2019 for material compatibility with AUS 32 DEF, ISO 179-1:2010 Charpy notched impact at −40°C, and ISO 16770:2004 full-notch creep ESCR. Published datasheet certification for this specific configuration is limited; converter validation against the OEM freeze-thaw protocol is normally required. Article types include 10-L, 20-L and 55-L portable tanks, 190-L wheeled fleet tanks, and marine DEF storage cassettes.
In the five-layer coextrusion of solvent-containing agrochemical adjuvants, HD5502W serves as the outer and inner skin layer, while the core EVOH barrier suppresses permeation of xylene, cyclohexanone and heavy aromatic naphtha. The layer split by mass is 55 ± 5 wt% HDPE skins, 28 ± 3 wt% post-industrial regrind core, 4 ± 1 wt% anhydride-modified tie layers, and 4 ± 1 wt% EVOH. The EVOH layer is held above 4 µm in the bottle sidewall to maintain solvent barrier; below this level, xylene permeation rises and the outer wall softens. Extrusion uses a 65-mm skin extruder (L/D 30:1) and a 35-mm barrier extruder (L/D 24:1) with a five-layer annular die at 215°C. Blow pressure is 0.8 MPa, and the mold is chilled to 15°C. The outer layer must not exceed 220°C melt temperature because EVOH residence time at the die then approaches its thermal degradation threshold, producing interfacial gels. Compliance follows UN 6.1 Packing Group III when the filled adjuvant is classified, with a drop height of 0.8 m; barrier layer quality is monitored by oxygen transmission according to ASTM D3985 on flat sheet and water vapor transmission according to ISO 15106-3. Finished article types include 1-L and 5-L bottles for xylene/cyclohexanone-based concentrates, 10-L crop oil methyl ester adjunct bottles, and 500-mL squeeze-and-measure dosing bottles.
Because residual ethyl acetate and toluene in printing ink and technical adhesive pails attack the container wall, the open-head pail body is extrusion blow molded from HD5502W without post-consumer recyclate. The compound is 100 phr HD5502W; 2.0 wt% carbon black masterbatch for black pails or 5.0 wt% TiO₂-based white masterbatch for water-based adhesive pails; 0.15 phr hindered phenolic antioxidant; and 0.1 phr calcium stearate. No post-consumer regrind is permitted, and internal regrind from punch-outs is limited to 10 wt% when the pail is destined for low-solvent fills. The body is blow molded on a 90-mm accumulator-head machine with L/D 24:1, melt temperature 195–210°C, mold temperature 15°C, and blow pressure 0.7 MPa. Top-load compression is verified by ISO 12048:2001 at 23°C; stackability of filled pails is tested at 40°C for 28 days when the contents are classified under EU CLP Regulation (EC) No 1272/2008 and assigned Packing Group III in transport. Finished article types include 5-L, 10-L, 15-L and 20-L open-head pails with lever-ring closures, 25-kg ink buckets, and 60-L paste pails with gasket-sealed lids.
Agricultural water storage containers in cold regions require a wall material that does not crack when partially filled and exposed to open-air thermal cycling. HD5502W has a density of 0.955 g/cm³ and a thin-section ductile-to-brittle transition well below −70°C, but sidewall notches at molded-in outlet bosses lower the practical service floor to −40°C. The formula is 100 phr HD5502W, 2.0 wt% UV-stabilized black or green concentrate, 0.2 wt% HALS, and 0.1 wt% processing stabilizer. No regrind is used when the tank is sold into regulated agricultural water systems; for nonpotable livestock wash-down, 20 wt% internal regrind is permitted. The tank is blown on a 120-mm accumulator-head machine with L/D 30:1, melt temperature 205–220°C, mold temperature 15–20°C, and blow pressure 0.8–1.0 MPa. Wall thickness at the outlet boss is programmed to 2.0 mm minimum; below that, drop impact at −40°C produces radial cracks from the threaded insert. Compliance testing includes Charpy notched impact according to ISO 179-1:2010, artificial weathering according to ISO 4892-2:2013, and restricted-substance screening under REACH Regulation (EC) No 1907/2006 Annex XVII. Finished products include 50-L, 75-L and 100-L vertical water storage tanks with threaded outlets, 20-L livestock dosing containers, and 30-L sprayer carry tanks. Potable-water certification is not claimed for this grade in all jurisdictions; the tanks are therefore designated agricultural and livestock service.
Competitive Sinopec Wuhan HDPE HD5502W prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Wuhan HDPE HD5502W is a high-density polyethylene blow-molding grade supplied by Sinopec Wuhan Petrochemical. The resin is used predominantly for extrusion blow molding of rigid containers, including detergent bottles, personal-care bottles, and small-to-medium industrial jerricans. Producer technical documentation lists a melt mass flow rate of 0.25 g/10 min at 190 °C and 2.16 kg load under ISO 1133-1:2022, and a density of 0.955 g/cm³ under ISO 1183-1:2019. These values place HD5502W among higher-molecular-weight HDPE blow-molding grades, which typically require elevated extruder head pressure but provide the parison melt strength needed for medium-to-large containers. Published data for specialized barrier or foamed configurations is limited.
| Property | Test method | Unit | Typical value |
|---|---|---|---|
| Melt mass flow rate, 190 °C, 2.16 kg | ISO 1133-1:2022 | g/10 min | 0.25 |
| Density, 23 °C | ISO 1183-1:2019 | g/cm³ | 0.955 |
| Tensile yield stress, 50 mm/min | ASTM D638-22 | MPa | 28 |
| Elongation at break | ASTM D638-22 | % | >600 |
| Flexural modulus, 2 mm/min | ASTM D790-17 | MPa | 1100 |
| Izod notched impact strength, 23 °C | ASTM D256-23 | kJ/m² | 20 |
| ESCR F50, 100 % Igepal CO-630, condition B | ASTM D1693-21 | h | >300 |
| Vicat softening temperature A50, 10 N | ISO 306:2022 | °C | 128 |
| Shore D hardness, 15 s | ISO 868:2003 | dimensionless | 64 |
The above values are typical lot averages from producer technical data sheets and are not guaranteed specification limits. On certificates of analysis, melt flow rate is often controlled within ±0.03 g/10 min at the 2.16 kg condition, and density within ±0.002 g/cm³. Such variation is small but measurable on a batch basis; for wall-thickness control in thin-walled containers, incoming resin lots should be tested using ISO 1133-1:2022 before extrusion parameters are fixed.
Rheologically, the grade exhibits shear thinning typical of high-molecular-weight HDPE. Capillary rheometry at 190 °C on comparable HDPE blow-molding resins shows apparent viscosity decreasing from approximately 950 Pa·s at 100 s⁻¹ to 210 Pa·s at 1000 s⁻¹; these values should be confirmed with lot-specific testing under ISO 11443:2021 before designing die gaps. The shear-thinning behavior allows complex mold geometries to be filled without excessive melt temperature, but it also means that small changes in screw speed can shift apparent viscosity and affect wall thickness distribution.
Extrusion blow molding of HD5502W on production lines typically uses barrel set points from 160 °C to 195 °C, with the die head held between 180 °C and 205 °C. In a continuous shuttle blow molder equipped with an 80 mm grooved-barrel extruder at L/D 30:1, steady-state melt temperatures of 188 °C to 193 °C have been recorded at screw speeds of 45 min⁻¹ to 60 min⁻¹. At die head temperatures above 210 °C, parison draw-down increases and surface oxidation may produce amber streaks; below 175 °C, die swell becomes erratic and the pinch-off weld line may exhibit roughness. A melt-temperature band of ±5 °C around the set point is therefore maintained by controlling screw speed, backpressure, and die head temperature. The parison programmer is adjusted to maintain wall-thickness variation no greater than 0.3 mm in the sidewall-to-pinch-off transition, particularly for container volumes above 5 L.
Mold temperature is normally held between 10 °C and 40 °C through closed-loop chillers. At the lower end of this range, cycle-time reduction of 8 % to 12 % is possible in thin-wall bottles, but the increased cooling rate reduces crystallinity and can lower top-load strength. At mold temperatures above 45 °C in thick-wall jerricans, warpage increases because cooling contraction becomes anisotropic between the flash pouch and the main body. Clamp force requirements in blow molding are lower than in injection molding; for a 5 L jerrican mold with a projected area of 0.09 m², a clamp force of 180 kN to 250 kN is usually sufficient.
Surface moisture on pellet surfaces is not a hydrolytic degradation risk for HDPE, but it can generate splay and microvoids in the parison. When pellets are stored in unheated silos at relative humidity above 60 %, hopper drying at 70 °C to 80 °C for 2 h to 4 h is applied. In coastal high-humidity plants, longer residence times are used, but drying air above 90 °C is avoided because static charge and pellet bridging become more severe. Dilute-phase vacuum conveying at velocities above 25 m/s can generate fines and angel hair in high-molecular-weight grades; dense-phase conveying below 10 m/s is preferred for preserving pellet geometry and feed stability. Feed throat flooding should be avoided because the low melt flow rate of HD5502W increases the sensitivity of grooved-barrel extruders to melt-pressure fluctuation when pellet intake is uneven.
HD5502W is not intended for thin-wall injection molding, film blowing, or pressure-pipe extrusion. Long-term hydrostatic strength ratings under ISO 9080:2022 should not be inferred from short-term burst or drop-impact data. End-use testing for aggressive liquids should follow ASTM D543-21, because strong oxidizing acids, aromatic hydrocarbons, and some chlorinated solvents can lower environmental stress-crack resistance. In applications involving prolonged diesel fuel contact, published data for this specific configuration is limited; qualification should include ESCR testing after fuel immersion rather than relying solely on as-molded resin values. Recycled-content incorporation should be validated for weld-line impact strength under ASTM D256-23 and for ESCR under ASTM D1693-21, because no universal blend ratio can be assigned without part-specific regression testing.
For long-term outdoor storage, carbon black masterbatch addition at 2.0 wt% to 2.5 wt% is used to meet weathering criteria under ISO 4892-2:2013. Without UV stabilization, HDPE loses impact strength and develops surface crazing within 6 months to 12 months in unprotected subtropical exposure. The exact stabilizer loading depends on part wall thickness and geographic UV index; accelerated weathering data should be generated for each container geometry.
Across the Wuhan HDPE portfolio, HD5502W differs from higher-flow blow-molding grades by its lower melt index and higher parison melt strength. Higher-flow grades with melt flow rates of 0.30 g/10 min to 0.50 g/10 min often run at lower extruder head pressure and allow shorter cycle times in small bottles, but they may require thicker nominal walls to pass drop-impact tests. Compared with bimodal pipe-grade HDPE, HD5502W is optimized for shear thinning and surface finish in intermittent parison extrusion rather than for long-term hydrostatic strength; bimodal pipe resins typically exhibit higher molar mass fractions and superior slow crack growth resistance under ISO 1167-1:2006. The selection boundary is therefore defined by the dominant failure mode of the final container: top-load, drop-impact, or stress-cracking.
When HD5502W is substituted for a general-purpose HDPE of higher melt flow rate, the extruder temperature profile is raised by 5 °C to 10 °C in the metering zone, and screw speed is reduced by 5 % to 15 % to maintain melt pressure below the machine limit. In a 1 L tight-neck bottle mold, the higher melt strength of HD5502W permits the parison programmer to reduce sidewall thickness from 1.0 mm to 0.8 mm while retaining top-load strength above 350 N under ASTM D2659-16. Cycle time may increase by 3 % to 8 % because of the lower melt flow rate, but the reduction in weight and improvement in drop-impact survival at -20 °C after 24 h conditioning justifies the substitution in detergent and personal-care packaging.
For industrial jerricans of 20 L to 25 L, accumulator head machines with a 1.5 kg to 2.5 kg shot capacity are used. Extruder output of 180 kg/h to 250 kg/h at screw speeds of 50 min⁻¹ to 70 min⁻¹ provides sufficient parison extrusion without exceeding melt temperature limits. A dropping height of 1.2 m at -18 °C is tested on filled containers according to ASTM D2463-15; HD5502W containers typically pass with no leak in the hinge and shoulder region when flash removal leaves a pinch-off tail height below 1.5 mm. Molds with post-cooling stations reduce cycle time by 10 % to 15 %, but the resin's low melt flow rate demands careful control of parison temperature at the pinch-off to avoid cold-weld defects.