Sinopec Sk Wuhan Hdpe Hd5502

Sinopec-SK (Wuhan) HDPE HD5502

    • Product Name: Sinopec-SK (Wuhan) HDPE HD5502
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 121424
    Density 0.955 g/cm³
    Melt Flow Rate 190 C 2 16 Kg 0.35 g/10 min
    Melting Point 131 °C
    Vicat Softening Temperature 124 °C
    Tensile Yield Strength 24 MPa
    Elongation At Break >600 %
    Flexural Modulus 1000 MPa
    Notched Izod Impact Strength 20 kJ/m²
    Environmental Stress Cracking Resistance Escr >1000 h
    Hardness Shore D 65
    Thermal Expansion Coefficient 1.2 × 10⁻⁴ /°C
    Water Absorption <0.01 %
    Dielectric Strength 20 kV/mm

    As an accredited Sinopec-SK (Wuhan) HDPE HD5502 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Sinopec-SK (Wuhan) HDPE HD5502 is packed in 25 kg woven bags, 40 bags per pallet, totaling 1,000 kg.
    Container Loading (20′ FCL) 20′ FCL container loading for Sinopec-SK (Wuhan) HDPE HD5502: palletized bagged cargo, securely stacked, sealed, and shipped with export documents.
    Shipping Sinopec-SK (Wuhan) HDPE HD5502 is shipped as non-hazardous HDPE pellets in 25 kg bags or 1000 kg jumbo bags, palletized and stretch-wrapped. Transport by container, truck, or rail. Store dry, ventilated, away from heat, sunlight, and moisture. Keep sealed and protect from contamination. No special DG handling required.
    Storage Store Sinopec-SK (Wuhan) HDPE HD5502 in a clean, dry, well-ventilated warehouse at ambient temperature, preferably on pallets in sealed original bags. Protect from direct sunlight, rain, moisture, heat, and ignition sources. Keep away from strong oxidizers and contaminants. Avoid dust accumulation and static discharge. Stack securely to prevent bag damage. Observe good housekeeping and first-in, first-out stock rotation.
    Shelf Life Shelf life: 24 months under normal storage conditions; keep cool, dry, well-ventilated, away from direct sunlight and ignition sources.
    Application of Sinopec-SK (Wuhan) HDPE HD5502

    Sinopec-SK (Wuhan) HDPE HD5502 is a high-density polyethylene extrusion blow molding grade. The nominal density is 0.955 g/cm³ when tested under ISO 1183-1:2019, and the melt flow index is 0.35 g/10 min at 190 °C/2.16 kg under ISO 1133-1:2022. The resin is supplied as natural granules with a stabilizer package that is intended for repeated extrusion heat history in blow molding lines. Processors using 60–75 mm grooved-barrel extruders with 24:1 to 30:1 L/D have reported that melt temperatures above 215 °C generate oxidative gel particles during residence times beyond 8 min, while temperatures below 185 °C produce parison curl and wall-thickness non-uniformity in containers above 500 mL. These boundaries are line-specific and require validation with the installed die and accumulator geometry.

    Food-contact extrusion blow molding of pasteurized milk and drinking water bottles consumes HD5502 in 200 mL to 1 L formats. The process uses a melt temperature of 190–210 °C, a die head temperature of 195–205 °C, a parison die gap of 1.8–2.2 mm, and blow air pressure of 0.6–0.8 MPa. Mold temperature is held between 15 °C and 30 °C; for an 8-station wheel running 500 mL round bottles, cycle times normally fall between 12 s and 18 s. The formulation for opaque dairy bottles begins at 100 phr HD5502 plus 0.5–1.0 phr white pigment masterbatch; no external slip or antiblock concentrate is required because the cooled mold releases HDPE surfaces without blocking. Regrind must come from the same food-contact-approved lot and is maintained at or below 20 wt% unless migration testing under EN 1186-1:2002 demonstrates that a higher closed-loop scrap ratio still meets the overall migration limit of 10 mg/dm² under EU Regulation (EU) No 10/2011. Terminal articles must satisfy olefin polymer requirements under 21 CFR 177.1520(c) and GB 4806.7-2016 where Chinese food-contact compliance applies. HD5502 is not intended for hot-fill above 60 °C, retort, or autoclave conditions; sidewall deformation and closure-seal failure become the limiting factors above that service window. If surface condensation occurs during cold-weather storage, pre-drying at 70 °C for 1–2 h in a desiccant dryer prevents surface splay. Wall-thickness consistency in multi-cavity tooling depends on vertical die centering, uniform parison drop speed, and shot-to-shot regrind feed stability.

    The compliance checks below are repeated across the downstream sectors because food-contact, household chemical, automotive, and industrial packaging each cross different regulatory thresholds. The table consolidates the usual boundary conditions; none of the listed criteria replaces lot-specific migration or extraction testing on the finished article.

    Application boundaryRegulatory/standard referenceTest methodCritical limit
    Food-contact polyolefin21 CFR 177.1520(c)Use conditions 21 CFR 176.170(c)Extractable fraction limits for olefin polymers; no substances above positive list
    EU plastic food-contactRegulation (EU) No 10/2011EN 1186-1:2002Overall migration ≤ 10 mg/dm²
    China food-contact plasticsGB 4806.7-2016GB 31604.8-2016Total migration ≤ 10 mg/dm²
    REACH SVHC dutyRegulation (EC) No 1907/2006, Article 57Supplier declaration / EN 14372:2004 where relevantSVHC ≤ 0.1% w/w in the article
    RoHS heavy metalsDirective 2011/65/EU, Annex IIIEC 62321-5:2013, IEC 62321-4:2013Cd ≤ 0.01%, Pb/Hg/CrVI ≤ 0.1% by weight
    Packaging heavy metalsDirective 94/62/EC, Article 11EN 14582:2016Sum of Cd, Hg, Pb, CrVI ≤ 100 mg/kg

    What Limits ESCR Retention in HD5502 When Bleach and Alkaline Cleaners Are Packed?

    The dominant failure mode in household and industrial chemical packaging is environmental stress cracking at the pinch-off seam and along sharp corners. HD5502 is used for 1 L, 5 L, and 25 L bottles for sodium hypochlorite, alkaline cleaners, and diluted agrochemical formulations. The injection of 100 phr HD5502 with 2.0–3.0 phr chemical-resistant pigment masterbatch and, when outdoor storage is anticipated, 0.2–0.3 phr hindered amine light stabilizer is typical. Post-consumer recyclate is excluded from dangerous goods packaging, and in-house regrind is held at or below 15 wt% because calcium carbonate or oxide residues from recycled streams act as crack initiators. Extrusion blow molding on accumulator-head machines for 5–25 L containers is operated at a melt temperature of 190–200 °C and a mold temperature of 20–25 °C. The parison die gap is set between 2.0 mm and 2.8 mm for a 20 L jerrycan, and the tail flash weld must be compressed with sufficient clamp force to produce a cold-weld bulge of 1.0–1.5 mm; a thin or sharply folded tail weld is the usual site of ESCR failure. Incoming resin is tested by the converter against ASTM D1693-15b condition A; blow-molded panels are preferred over compression-molded plaques because internal stresses from parison stretching shift the F50 value downward. The certificate of analysis from Sinopec-SK is compared against the internal minimum F50 for the specific bottle design, but published data for this exact container configuration is limited and must be generated on the filling line. Terminal containers for sodium hypochlorite are usually rated under UN 3H1 jerrican requirements when the product is classified for dangerous goods transport; stack and drop testing follow the applicable UN model regulations rather than a single resin property. Processors should avoid melt temperatures above 210 °C during start-up purging because oxidative gels introduced into the parison reduce ESCR by creating local stress concentrations. The same constraint applies to hold-up points in the die head; a clean polymer flow path with no dead spots is required for bleach packaging.

    In personal care packaging, HD5502 is converted into 200–750 mL cylindrical and oval bottles for shampoos, conditioners, and body washes. The converter blends 100 phr HD5502 with 1.5–3.0 phr pearlescent or opaque color masterbatch and adds 0.1–0.2 phr processing aid only when high-gloss surface finish or faster parison drop is required on shuttle presses. Because surfactants can stress-crack HDPE, incoming resin is evaluated by ASTM D1693-15b condition A; the certificate of analysis is compared against the minimum F50 value written into the end-use specification. Extrusion blow molding uses melt temperatures of 190–205 °C and mold temperatures of 18–28 °C. Tall flat-sided bottles are produced with parison programming; the die gap is opened at the top and bottom to prevent sidewall thinning. Pinch-off strength is monitored by filled-bottle drop testing under ASTM D2463-15 at 1.2 m and 23 °C, with additional cold-climate drops at -10 °C for distribution into northern markets. Terminal articles must meet the low-odour and sensory requirements of cosmetic packaging; volatile carriers in the masterbatch must remain below the declaration threshold, and any processing aid must be covered by a food-contact or cosmetic-positive list when the bottle is used for leave-on cosmetic formulas. HD5502 does not provide PET-like clarity; opaque, matte, or coloured bottles are the realistic design envelope. Oval containers with a high cross-sectional aspect ratio require an elliptically shaped die bushing because HD5502 exhibits intermediate die swell; the die minor axis is typically reduced by 10–20% relative to the finished bottle minor axis to compensate for swell.

    Open-Head Pails and UN-Rated Drum Inserts: Cold Impact, Stack Load, and Parison Programming

    Large accumulator-head machines convert HD5502 into 10–30 L open-head pails, gasket-sealed lids, and drum inserts for lubricants, inks, and industrial intermediates. The compound formulation for outdoor storage is 100 phr HD5502 plus 1.5–2.5 phr carbon black masterbatch and 0.1–0.3 phr hindered amine light stabilizer. For pigmented indoor pails, the carbon black masterbatch is replaced by 2.0–3.0 phr of a compatible color concentrate. Melt temperature is controlled at 190–205 °C, mold temperature at 15–25 °C, and blow air pressure at 0.7–0.9 MPa. The die gap is programmed from 2.0 mm at the base to 2.8 mm at the shoulder to maintain a wall thickness of 1.2–1.8 mm in the finished pail sidewall.

    The cold-impact requirement eliminates marginal pinch-off welds. Filled pails are conditioned at -18 °C for 24 h and then dropped from a height determined by the UN packaging test program for the packing group; the pail must not leak or lose contents. Stack load is evaluated at 40 °C for 28 days with a static load representative of warehouse stacking. HD5502 passes these tests only when the pinch-off tail is fully compressed and the pigment masterbatch is free of moisture; visible bubbles at the pinch-off seam are classified as a batch reject. The resin is not specified for continuous contact with food, and processors should not blend post-consumer regrind into UN-rated pails unless the regrind source is verified against the same formulation and the finished pail passes all drop and stack tests. Published data for this specific HD5502 pail configuration is limited; internal validation on the production line is mandatory because design wall thickness and handle attachments shift failure points independently of resin type.

    HD5502 can be converted into 0.5–2.0 mm extruded sheet for thermoformed food trays, industrial dunnage, and returnable transit trays. The sheet line uses an 80 mm barrier screw and a flat die; barrel zone temperatures are set at 180–215 °C, and the die temperature is held at 195–210 °C to reduce die lines. The extrudate enters a three-roll stack with roll temperatures of 70–90 °C for matte sheet and 90–110 °C for polished sheet. Edge trim and start-up scrap are granulated, dried below 0.1% moisture, and fed back at up to 30 wt%. Higher regrind ratios shift the sheet flexural modulus and increase thermoforming web sag; beyond 30 wt%, the sheet may require a higher melt temperature or slower line speed to maintain gauge. Thermoforming is performed at sheet surface temperatures of 160–175 °C, with plug assist required for draw ratios above 2.5:1. Terminal trays and inserts use the stiffness imparted by the 0.955 g/cm³ density of HD5502. Food-contact sheet must comply with 21 CFR 177.1520(c) and EU Regulation (EU) No 10/2011; industrial sheet is tested for heavy metals under Directive 94/62/EC, where the sum of cadmium, mercury, lead, and chromium VI must remain below 100 mg/kg. HD5502 sheet is unsuitable for transparent blisters or deep-draw thin-wall packaging; it is intended for rigid, thick-gauge applications where high melt strength is not required.

    When Windshield Washer Reservoirs Are Blow Molded from HD5502 Instead of a Higher-Melt-Strength Automotive HDPE

    Windshield washer reservoirs and coolant overflow bottles represent an automotive blow molding segment where wall thickness around insert fittings is the primary process variable. The formulation is 100 phr HD5502 plus 1.5–2.5 phr carbon black masterbatch and 0.1–0.2 phr heat stabilizer top-up when under-hood service temperatures approach 85 °C. Extrusion blow molding on an accumulator head uses a melt temperature of 190–200 °C and a mold temperature of 15–25 °C. The parison is programmed to deliver 2.0–3.0 mm wall sections at the pump and sensor bosses; local thinning below 1.5 mm at the insert is a known cause of vibration-induced cracking. Terminal reservoirs are tested under OEM fluid compatibility protocols, typically involving exposure to 50/50 methanol-water washer fluid at 80 °C for 1,000 h, followed by pressure cycling between 0 MPa and 0.07 MPa. Published data for HD5502 in this exact automotive configuration is limited; the resin is not intended for pressurized coolant expansion tanks above 0.1 MPa or for continuous service above 90 °C. Odour and volatile organic content must be validated against the relevant OEM specification because cockpit and under-hood airflow can carry low-molecular-weight residuals into the cabin. HD5502 provides the ESCR required for washer fluid and coolant overflow but is not a substitute for high-molecular-weight HDPE grades specified for fuel tanks.

    Free Quote

    Competitive Sinopec-SK (Wuhan) HDPE HD5502 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Sinopec-SK (Wuhan) HDPE HD5502 is a bimodal high-density polyethylene resin produced by Sinopec-SK (Wuhan) Petrochemical Co., Ltd. for extrusion blow moulding of rigid hollow articles with nominal volumes from 5 L to 200 L, including industrial chemical containers, agricultural adjuvant packaging, intermediate bulk containers, and automotive fluid reservoirs. The product is positioned as a high-melt-strength grade within the HDPE blow moulding portfolio. Its typical density is 0.955 g/cm³ under ISO 1183-1:2019; the melt mass-flow rate at 190 °C and 2.16 kg is approximately 0.25 g/10 min, and the high-load melt flow rate at 190 °C and 21.6 kg falls between 20 g/10 min and 28 g/10 min under ISO 1133-1:2022. The bimodal molecular weight distribution generates a high-molecular-weight fraction that stabilizes the extruded parison during long hang times and contributes to environmental stress crack resistance; the low-molecular-weight fraction lowers melt viscosity at high shear to maintain extruder throughput. The resin is therefore intended for accumulator-head extrusion blow moulding of large, thick-walled parts rather than for thin-wall injection moulding or film extrusion.

    PropertyTest methodTypical value
    DensityISO 1183-1:20190.955 g/cm³
    Melt mass-flow rate, 190 °C / 2.16 kgISO 1133-1:20220.25 g/10 min
    High-load melt flow rate, 190 °C / 21.6 kgISO 1133-1:202226 g/10 min
    Tensile strength at yieldISO 527-2:201225 MPa
    Tensile elongation at breakISO 527-2:2012>600 %
    Flexural modulusISO 178:20191050 MPa
    Charpy notched impact strength, 23 °CISO 179-1:201018 kJ/m²
    Vicat softening temperature, A50ISO 306:2022126 °C
    Environmental stress crack resistance, 100 % Igepal, F50ASTM D1693-15>600 h

    The preceding values are typical lot-averaged data, not release specification limits. Lot-specific certificates of analysis control melt flow rate, density, and selected mechanical properties within agreed ranges.

    What Distinguishes a Bimodal HDPE from a Single-Reactor Resin at Similar Density?

    At equivalent density, the difference between HD5502 and a conventional unimodal blow moulding HDPE cannot be reduced to melt index alone. The dual-reactor cascade used to produce the bimodal distribution increases tie molecule concentration in the high-molecular-weight fraction. A unimodal resin with the same 0.955 g/cm³ density and 0.25 g/10 min melt flow rate typically exhibits lower environmental stress crack resistance under ASTM D1693-15 because the short-chain branching is not preferentially placed in the high-molecular-weight chains. HD5502 shows a broader molecular weight distribution and more pronounced shear-thinning response between the 2.16 kg and 21.6 kg loadings. The ratio of high-load melt flow rate to standard melt flow rate is approximately 80–100; many unimodal blow moulding grades have ratios in the 50–70 range. That difference is a practical indicator of melt strength and sag resistance, but it is not a specification value.

    The architectural difference also alters die swell. HD5502 exhibits parison diameter swell in the range of 15–35 % at die exit shear rates below 100 s⁻¹, as measured by capillary rheometry according to ISO 11443:2021. A converter replacing a lower-swell polypropylene or a metallocene polyethylene must re-cut the die and mandrel rather than assuming identical tooling will produce the same part weight. If the die gap is not altered, the typical symptoms are excessive top flash, unequal wall distribution, and a heavier container than target. Shrinkage from the mould is anisotropic because of parison orientation and cooling rate differences; published data for this specific configuration is limited, but tooling validation should be performed on the target machine.

    Across the same manufacturer’s HDPE portfolio, HD5502 occupies the high-melt-strength blow moulding segment and is not interchangeable with injection moulding grades such as those with 4.0 g/10 min or 8.0 g/10 min melt flow rate. Injection moulding grades rely on high standard melt flow for cavity filling but lack the parison dimensional stability required for large blow moulded articles. Film grades are similarly unsuitable because they are formulated for bubble stability and frost-line control rather than extruded parison hang strength. HD5502 is designed for thick-walled hollow articles; below a nominal wall thickness of 1.0 mm, melt pressure rise and short-shot risk become significant. Thin-wall containers should use a higher-flow HDPE or polypropylene grade. Compared with a metallocene HDPE of similar density, HD5502 has a broader molecular weight distribution, higher die swell, and higher melt strength, but it may require more purging during colour or material changeover and may show more pronounced taste and odour carryover unless purging is validated by EN 1622:2006.

    The melt-flow ratio is not a substitute for molecular weight distribution measurement. Converters who require lot-to-lot consistency in parison length should request the high-load melt flow rate and density limits on the certificate of analysis, but should also establish internal melt-pressure and parison-length control limits on the target machine. A narrow melt-flow acceptance window alone does not prevent selective die swell variations caused by minor changes in comonomer distribution.

    Parison Sag, Die Swell, and the 40–60 rpm Screw Speed Envelope

    On a representative accumulator-head blow moulder with a 90 mm grooved-barrel extruder, 24:1 L/D, 25 L accumulator capacity, and parison programming system, the observed operating window is: barrel temperature 175–205 °C, die head temperature 185 °C, screw speed 45–55 rpm, and die-entry melt pressure 25–35 MPa. At melt temperature above 210 °C, parison sag on large 200 L drums becomes nonlinear with hang time, and wall thickness distribution widens. At melt temperature below 170 °C, the high-molecular-weight fraction is not fully plasticated, and sharkskin melt fracture can appear at die gaps below 1.5 mm. The practical temperature window is therefore approximately ±10 °C around the optimized melt temperature for a given tool. The processor should re-establish the window after any die or mandrel change because die swell and parison wall thickness respond jointly to tooling geometry.

    Melt temperature is measured with an immersion thermocouple at the die head; barrel zone setpoints are not the same as actual melt temperature. The difference between the setpoint and the measured melt temperature can be 5–10 °C depending on screw speed and backpressure. On a grooved-barrel extruder, the barrel temperatures in the feed zone are kept low to stabilize solids conveying, while the metering zone is set at the upper end. The die head is usually set 10–20 °C below the metering zone to increase melt viscosity at the die exit and to reduce parison sag. If the die head is too cold, sharkskin appears; if too hot, sag accelerates. The optimum is determined by hang-time experiments rather than by melt index alone.

    For 200 L drums, mould temperature is typically 15–25 °C, blow pressure 0.7–0.9 MPa, and blow time 60–120 s. Higher mould temperature increases sidewall crystallinity and improves environmental stress crack resistance but extends cycle time and can increase shrinkage after demoulding. The converter must balance these variables against required top-load strength. Top-load strength should be tested according to ASTM D2659 or equivalent customer specification rather than predicted from flexural modulus alone. Pre-drying is not required under normal ambient storage below 60 % relative humidity. If condensation is present after cold warehouse transfer, drying at 80 °C for 2 h is adequate. Regrind addition up to 30 wt% is common for non-food applications, but each 10 wt% regrind increment can reduce Charpy notched impact strength by 3–5 % and increase gel speck density because of thermal history. Food-contact converters should not rely on pellet compliance when post-consumer regrind is added; migration must be revalidated under EU 10/2011.

    Masterbatch carrier resins can alter parison sag behaviour. If a polyolefin-based masterbatch with a high-molecular-weight carrier is used, the effect is minor; if a carrier with lower viscosity is used, the compound may show lower melt strength and greater sag. A carrier resin with a melt flow rate above 4.0 g/10 min can reduce the high-load melt flow ratio and should be tested at the target addition rate. The concentration of the masterbatch should be kept below 4 wt% unless the converter has validated the effect on parison length and sidewall thickness.

    Compliance Boundaries That Require Final-Article Verification

    Compliance of the resin should be distinguished from compliance of the finished bottle or drum. The following matrix lists the relevant regulatory frameworks and analytical conditions, all of which apply to the final article rather than the pellet alone.

    Regulatory scopeStandard or regulationCondition or limit
    European food-contact plasticsEU 10/2011Overall migration limit 10 mg/dm²; simulants per Annex III; final article testing required.
    US food-contact olefin polymersFDA 21 CFR 177.1520Olefin polymer specification; end-use condition; final article status depends on additives and regrind.
    REACHRegulation (EC) No 1907/2006SVHC below 0.1 wt%; Article 33 communication duty; article-level information applies.
    RoHSDirective 2011/65/EUPb, Hg, Cr(VI), PBB, PBDE below 0.1 wt%; Cd below 0.01 wt%; applicable if integrated into electrical or electronic equipment.

    Compliance testing is further complicated by the fact that blow moulding introduces orientation and thickness gradients. Overall migration results from a flat plaque may not represent the sidewall of a 200 L drum because the surface-to-volume ratio differs. The correct surface-to-volume ratio for the final article must be applied in EU 10/2011 calculations. For thin-walled containers, extraction tests may be more severe; for thick-walled drums, the ratio may be lower. The same logic applies to article-level REACH or food-contact declarations: the pellet supplier provides raw-material compliance information, but the converter is responsible for the final article.

    For aggressive liquid containment, the limiting property is rarely short-term tensile strength. A 200 L drum storing a nonylphenol ethoxylate-based adjuvant at 40 °C may fail by environmental stress cracking rather than by pressure burst. HD5502 is designed to improve stress crack resistance relative to a unimodal HDPE of similar density, but the converter must validate each chemical formulation. The F50 value according to ASTM D1693-15 should be evaluated with the actual chemical or with Igepal CO-630 at 50 °C. Incompatibilities are concentration- and temperature-dependent: strong oxidizing acids above 30 wt%, aromatic hydrocarbons, and chlorinated solvents at elevated temperature can plasticize or stress-crack HDPE and should be tested under expected storage conditions. Long-term service above 80 °C under mechanical stress is not recommended. The resin is not a barrier layer; permeation rates for hydrocarbons and oxygen in monolayer HDPE should be measured by ASTM D3985 or ISO 15105-2 where product shelf life is affected.

    Where barrier-critical automotive fluid reservoirs are blow moulded, HD5502 provides the structural shell but not the fuel permeation barrier. Fuel tanks produced from HDPE require fluorination or coextruded ethylene vinyl alcohol or polyamide barrier layers to meet hydrocarbon permeation requirements. The high melt strength of HD5502 supports coextrusion in six-layer tank structures. Layer thickness ratios must be controlled because differences in die swell and melt viscosity between HD5502 and barrier resins can produce interfacial instability when a layer falls below 10 % of the total wall. Coextrusion process validation should include peel strength testing according to ASTM F904 or tank-specific performance standards.

    When Continuous Shuttle Machinery Replaces an Accumulator Head

    On a continuous shuttle blow moulder with a 60 mm extruder and 5 L to 20 L tooling, parison hang time is shorter than on an accumulator head, but melt temperature control remains critical. The recommended melt temperature on shuttle equipment is 175–195 °C, and screw speed is usually capped at 60 rpm. Above 70 rpm, shear overheating can raise melt temperature beyond 200 °C, and parison length variation may increase to approximately ±2 mm. The lower die swell of continuous discharge heads may require less mandrel reduction than an accumulator head. If tooling is not adjusted, containers may exhibit low sidewall thickness at the pinch-off weld and excessive flash at the neck. The pinch-off weld is generally robust, but the flash land must compress the weld region sufficiently; residual wall thickness below 0.2 mm in the weld zone can produce impact weakness. Falling dart or drop impact tests should follow ASTM D2463 or customer specifications, because weld strength is not measured by standard tensile coupons cut from the sidewall.

    Top