| HS Code | 132980 |
| Product Name | Sinopec Sichuan HDPE HMCRP100N |
| Polymer Type | High Density Polyethylene (HDPE) |
| Grade | PE100 |
| Density | 0.949 g/cm³ |
| Melt Flow Rate 190 C 5 0 Kg | 0.20-0.23 g/10 min |
| Tensile Yield Strength | ≥25 MPa |
| Elongation At Break | ≥600% |
| Flexural Modulus | ≥1000 MPa |
| Notched Izod Impact Strength 23 C | ≥30 kJ/m² |
| Vicat Softening Temperature | ≥125°C |
| Oxidation Induction Time 200 C | ≥20 min |
| Environmental Stress Cracking Resistance | ≥5000 h |
| Melting Point | 130-135°C |
| Mrs | 10.0 MPa |
| Color | Natural |
| Form | Pellets |
As an accredited Sinopec Sichuan HDPE HMCRP100N factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinopec Sichuan HDPE HMCRP100N is packaged in 25 kg woven bags, 40 bags per pallet (1,000 kg). |
| Container Loading (20′ FCL) | Sinopec Sichuan HDPE HMCRP100N loaded into a 20′ FCL, typically 25 MT palletized or 28 MT unpalletized, secured for export. |
| Shipping | Sinopec Sichuan HDPE HMCRP100N ships as a non-hazardous thermoplastic resin, typically in 25 kg PP woven bags, about 25 MT per 20'FCL, palletized or bulk. Store cool, dry, ventilated; protect from sunlight, moisture, contamination, and physical damage. Not classified as dangerous goods for transport. Keep away from ignition sources. |
| Storage | Store Sinopec Sichuan HDPE HMCRP100N in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and strong oxidizers. Keep original bags or containers closed, palletized off the floor, and protect from moisture, dust, and contaminants. Avoid prolonged UV exposure. Use stable stacking, maintain first-in-first-out rotation, and follow local safety regulations. Store away from acids, bases, and incompatible materials. |
| Shelf Life | Shelf life is typically 12 months from production date when stored in original packaging, dry, cool, and away from direct sunlight. |
In potable water main extrusion, Sinopec Sichuan HDPE HMCRP100N is introduced at the feed throat as a dry blend with carbon black masterbatch at 2.0–2.5 wt%, a loading required for UV-stabilized black pipe under ISO 4427-1 and EN 12201-1. The finished pipe is dimensioned to SDR 11 for a 16 bar pressure rating or SDR 17 for a 10 bar rating at 20 °C, based on the PE100 design stress of 8 MPa derived from an MRS of 10 MPa per ISO 9080 and ISO 12162. Extrusion is performed on a grooved-feed single-screw extruder with L/D 30:1 to 36:1, using barrel set points from 190 °C to 230 °C. Melt temperature above 230 °C reduces the oxidation induction time and shifts the long-term hydrostatic failure mode. The vacuum calibration tank is held at 15–30 °C to balance dimensional shrinkage against residual stress. Screen packs of 60 mesh over 100 mesh are used to protect the die from fines. Field-scale output limits are typically governed by melt-pressure instability at the screen pack rather than motor load, particularly when upstream regrind contains pipe trim with variable bulk density. Desiccant drying is not required because HDPE is not hygroscopic, but hopper hot-air drying at 70–80 °C is used when surface condensation is visible above 70% relative humidity. The resulting product is black pressure pipe for municipal drinking water networks, service laterals, and rural water supply headers. Final pipe assemblies are subjected to ISO 1167-1 hydrostatic testing after butt fusion.
For buried gas mains, the governing standard shifts from water-specific requirements to ISO 4437-2, and the pipe is usually produced with a yellow outer layer or yellow stripes on a black base. HMCRP100N is again loaded with 2.0–2.5 wt% carbon black masterbatch, but the decisive extrusion control is not hydrostatic strength alone. The finished wall must also pass rapid crack propagation resistance under ISO 13477 at 0 °C and notched-pipe slow crack growth under ISO 13479. The slow crack growth threshold is sensitive to gel dispersion and residual stress, so barrel temperature profile is kept within 200–225 °C and die gaps are set to avoid excessive draw-down. On production-scale lines, high screw rpm can create local melt-temperature overshoot and surface melt fracture at the outer wall. Such defects are not accepted because they act as crack initiation sites at butt-fusion welds. Butt-fusion joining is qualified to ISO 21307, with weld bead geometry checked per ISO 13953. The terminal products are below-ground natural gas distribution mains and service laterals with pressure rating selected by utility specifications, frequently SDR 11 or SDR 17 depending on maximum operating pressure.
Mineral slurry transport with HMCRP100N pipe does not require potable water or gas certifications. Instead the design is governed by abrasion allowance and pressure surge. Pipe is normally extruded as SDR 13.6 or SDR 11 black pipe with 2.0–2.5 wt% carbon black, and butt-fusion welds are made with full external bead removal in coarse-particle services. Slurry velocity is kept between 2.5 m/s and 4.5 m/s. Below 2.5 m/s, solids settle and create bottom-wall wear. Above 4.5 m/s, high-silica abrasion accelerates wall loss. The HDPE pipe provides corrosion resistance in acidic tailings water but has a lower absolute wear index than ceramic-lined steel. Wall-thickness monitoring by ultrasonic gauges at elbows is therefore standard practice. Published wear-rate data for this specific resin under high-silica slurry is limited. Material selection relies on comparative abrasion tests in the actual slurry rather than extrapolated coupon data. Terminal products include tailings headers, dredge discharge lines, and process water return lines in mining and mineral processing plants.
Non-pressure corrugated duct for underground power and fiber optic cable is a lower design-intensity use of HMCRP100N. The resin is extruded with 2.0–2.5 wt% carbon black for UV resistance and formed into corrugated or smooth-wall conduit under EN 61386 or UL 651. Ring stiffness is verified according to ISO 9969. No hydrostatic design stress is required, but the PE100 molecular architecture is used because it allows thin-wall corrugations to survive installation crush and backfill loads. The terminal product is underground cable duct for telecommunications and low-voltage electrical distribution.
Closed-loop ground-source heat pump circuits are extruded as SDR 11 or SDR 17 black pipe and are normally limited to fluid temperatures below 40 °C. Above this threshold, long-term hydrostatic strength is derated according to ISO 4427-1 temperature-pressure curves. The process-critical defect in geothermal loops is a butt-fusion bead notch at the inner diameter. Such a notch can act as a slow crack initiation point under cyclic thermal expansion and soil movement. Fusion procedures are therefore controlled to ISO 21307, and the pipe inside diameter tolerance is maintained within ±0.5 mm for socket fusion compatibility. The finished geothermal loop is pressure-tested before backfill at 1.5 times the design operating pressure. Terminal products are vertical and horizontal ground loops for residential, commercial, and district-scale ground-source heat pump systems.
Trenchless sliplining and pipe bursting with HMCRP100N liner pipe places the main design load on external annular pressure and insertion pull force rather than internal hydrostatic pressure. Liner wall thickness is selected according to ASTM F1216 or AWWA M55 guidance for collapse resistance. Butt-fused strings are pulled through the host pipe with reduction dies that temporarily reduce outside diameter by up to 6%. Pull force must remain below the fused joint tensile capacity. The PE100 long-term strength allows SDR 17 to SDR 26 liner pipes to withstand external groundwater head after annular grouting. The limiting operational boundary is the allowable insertion pull distance and the acceptable surface scoring depth. Terminal products are renewed potable water and gravity sewer liners installed inside deteriorated concrete or metallic pipelines.
| Application segment | Core standards | Carbon black loading | Pressure or design class |
|---|---|---|---|
| Potable water mains | ISO 4427-2; EN 12201-2; NSF/ANSI/CAN 61 | 2.0–2.5 wt% | PN 16 (SDR 11); PN 10 (SDR 17) |
| Gas distribution | ISO 4437-2; ISO 13477; ISO 13479 | 2.0–2.5 wt% | Utility-specified MOP |
| Mineral slurry and tailings | ISO 4427-2; ISO 21307 | 2.0–2.5 wt% | SDR 13.6; SDR 11 |
| Cable duct and conduit | EN 61386; UL 651; ISO 9969 | 2.0–2.5 wt% | Non-pressure |
| Geothermal ground loops | ISO 4427-1; ISO 21307 | 2.0–2.5 wt% | SDR 11; SDR 17 |
| Trenchless rehabilitation liner | ASTM F1216; AWWA M55 | 2.0–2.5 wt% | SDR 17–SDR 26 |
Competitive Sinopec Sichuan HDPE HMCRP100N prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Sichuan HDPE HMCRP100N is classified as a bimodal high-density polyethylene resin intended for pressure pipe extrusion. Manufacturer technical data for the grade report a density of 0.949–0.953 g/cm³ when determined by ISO 1183-1:2019 and a melt mass-flow rate of 0.20–0.28 g/10 min at 190 °C/5 kg according to ISO 1133-1:2022. Under ISO 9080:2012 pipe-grade extrapolation, the material is designed to satisfy the PE100 minimum required strength of 10.0 MPa at 20 °C for 50 years. Additional datasheet values include tensile yield stress of 22–25 MPa under ISO 527-2:2012, elongation at break above 500%, Vicat softening temperature of 124–127 °C under ISO 306:2022, and oxidation induction time above 20 min at 200 °C under ISO 11357-6:2018.
Independent control of hydrogen and comonomer concentration in the two polymerization reactors permits the bimodal molecular weight distribution that defines this grade. The low-molecular-weight fraction contains limited short-chain branching and contributes shear thinning, while the high-molecular-weight fraction incorporates most of the comonomer and supplies the tie-molecule population needed for slow crack growth resistance. Gel permeation chromatography of this resin class typically yields a polydispersity index between 15 and 25, compared with 4–8 for many single-reactor high-density polyethylene grades. The practical consequence is that HMCRP100N cannot be evaluated by melt mass-flow rate alone; apparent viscosity at pipe-extrusion shear rates is substantially lower than predicted from the 5 kg MFR.
The high-molecular-weight tail increases the number of tie molecules spanning adjacent crystalline lamellae. In notched pipe testing under ISO 13479:2009, specimens are held at 80 °C under internal pressure to accelerate brittle failure. Resins with a sufficiently broad bimodal distribution exhibit extended stable crack propagation times because the tie molecules resist craze fibril rupture. At the same time, the low-molecular-weight fraction reduces viscosity at high shear rates. Capillary rheometry data for bimodal pipe grades measured under ISO 11443:2021 show shear stress at 100 s⁻¹ and 190 °C that is typically 20–35% lower than for a unimodal resin of similar weight-average molecular weight. This allows higher output before reaching the die-head pressure limit.
Differential scanning calorimetry under ISO 11357-3:2018 usually displays a main melting endotherm between 130 °C and 135 °C with a lower-temperature shoulder from the comonomer-rich high-molecular-weight fraction. The shoulder is not a processing defect; it reflects the deliberate placement of short-chain branches in the high-molecular-weight species. Pipe extruders that attempt to eliminate this shoulder by raising melt temperature above 230 °C instead accelerate stabilizer consumption, reduce oxidation induction time, and may generate surface shark-skin and die-lip build-up.
Pressure rating calculations for water and gas pipelines follow the ISO 4427 and ISO 4437 series. For PE100 materials, the design stress is 8.0 MPa when a design coefficient of 1.25 is applied to the 10.0 MPa minimum required strength specified in ISO 12162:2009. PE80 grades use 6.3 MPa under the same coefficient. Consequently, a PE100 pipe can be rated at 16 bar with a standard dimension ratio of 11, whereas a PE80 pipe typically achieves 12.5 bar at the same SDR. The wall-thickness reduction for equivalent pressure class lowers material consumption and increases hydraulic bore capacity. However, the thinner wall concentrates stress around carbon black agglomerates; carbon black dispersion must therefore be controlled to a rating of ≤3 under ISO 18553:2002 when a black compound is specified.
In practice, the wall-thickness reduction from PE80 to PE100 imposes stricter demands on pipe calibration and vacuum sizing. A 16 bar PE100 pipe at SDR 11 has less melt mass per unit length, which reduces cooling time but narrows the processing window for roundness and wall-thickness distribution. Ultrasonic wall-thickness scanning at 8–16 measurement points around the circumference is used to verify that minimum wall thickness does not fall below the value required by ISO 4427-2:2019. Failure to maintain uniform wall thickness produces local stress concentrations that invalidate the hydrostatic design basis, even if the compound itself meets PE100 requirements.
The table below summarises representative property windows from public datasheets for bimodal PE100 pipe resin and conventional PE80/single-reactor high-density polyethylene references. Values are not lot guarantees; the certificate of analysis for a specific shipment takes precedence.
| Property | Test method | HMCRP100N typical window | PE80 reference window |
|---|---|---|---|
| Density at 23 °C | ISO 1183-1:2019 | 0.949–0.953 g/cm³ | 0.941–0.948 g/cm³ |
| Melt mass-flow rate 190 °C/5 kg | ISO 1133-1:2022 | 0.20–0.28 g/10 min | 0.40–0.80 g/10 min |
| Tensile yield stress | ISO 527-2:2012 | ≥22.0 MPa | ≥18.0 MPa |
| Minimum required strength | ISO 9080:2012 / ISO 12162:2009 | 10.0 MPa | 8.0 MPa |
| Oxidation induction time 200 °C | ISO 11357-6:2018 | ≥20 min | ≥20 min |
| Carbon black dispersion rating | ISO 18553:2002 | ≤3 | ≤3 |
The lower melt mass-flow rate of HMCRP100N should not be interpreted as a processing deficiency. The bimodal distribution raises the shear-thinning exponent, so apparent viscosity at extrusion shear rates can be comparable to a PE80 grade with a higher MFR. Pipe-grade qualification relies on notched pipe tests such as ISO 13479:2009 rather than coupon-level ESCR analysis, because pipe-wall stress states reproduce service conditions more accurately. Coupon-level environmental stress crack resistance under ASTM D1693-15e1 can exceed 1,000 h for bimodal PE100 grades, but that result alone is not sufficient for pipe certification.
On production-scale grooved-feed lines running 450–630 mm pipe, output limitations are not governed solely by screw design. At high screw speeds above 110–130 rpm, shear heating in the compression zone can raise measured melt temperature by 8–15 °C above barrel setpoint. Operators may compensate by lowering rear barrel zones to 180 °C while maintaining die zones at 215 °C, but this practice increases torque and can destabilize the melt seal. A screen pack of 20/40/60 mesh raises head pressure by 3–6 MPa and improves carbon black dispersion, yet the additional shear work narrows the remaining melt-temperature safety margin. The preferred control strategy is to monitor melt temperature with an immersion probe at the adapter and limit throughput so that the probe reading remains below 228 °C. Published data for this specific configuration is limited; the numerical ranges are compiled from typical PE100 bimodal extrusion bulletins and should be confirmed on the target line.
Admixtures of peroxide-containing compounds, silane-grafted polyethylene scrap, or polypropylene at mass fractions greater than 2 wt% are incompatible with the intended molecular architecture. Peroxide residues initiate long-chain branching and gel formation, appearing as surface pimples and melt fracture during extrusion. Silane-grafted scrap raises melt elasticity and can destabilize spiral or cone flow in the die, producing weld-line weakness in thick-walled pipe. Polypropylene contamination above 2 wt% depresses slow crack growth resistance and can create delamination planes under sustained internal pressure. These boundaries should be verified by melt filtration pressure rise, extrusion surface inspection, and fracture-surface microscopy before converting a line that previously processed general-purpose HDPE.
Quality assurance for pipe-grade release includes density, melt mass-flow rate, tensile yield stress, carbon black dispersion, oxidation induction time, and hydrostatic pressure testing. Lot-to-lot variance in bimodal resins is often detected by monitoring the melt flow ratio and dynamic rheology crossover frequency. A downward shift in the high-molecular-weight fraction increases melt flow and reduces slow crack growth resistance, while an upward shift raises die pressure and may trigger melt fracture. The manufacturer certificate of analysis should be compared against internal control limits established during line qualification.
In potable-water service, finished pipes produced from this resin must be assessed under the relevant national health agency framework. The resin alone does not carry final pipe certification. In European practice, pipe systems are evaluated under local test protocols such as BS 6920-1:2014 or the applicable German KTW guideline. For gas service, ISO 4437-2:2014 specifies requirements for PE pipes, including rapid crack propagation testing under ISO 13477:2008. In China, corresponding water and gas pipe standards are GB/T 13663.2-2018 and GB 15558.1-2015. Systems requiring continuous exposure above 60 °C or contact with strong oxidizing agents should be reassessed against chemical resistance tables, because high-density polyethylene undergoes accelerated oxidative degradation under combined thermal and chlorine stress.
Compared with PE80, the primary difference is not density but the long-term hydrostatic strength curve. HMCRP100N-class PE100 material achieves the same design stress at reduced wall thickness because the high-molecular-weight fraction suppresses slow crack growth. Compared with single-reactor HDPE used for blow molding or film, the melt index under 2.16 kg is significantly lower, typically below 0.10 g/10 min, and melt strength is insufficient for large-part blow molding. The resin is therefore not interchangeable with general-purpose HDPE in applications requiring high flow or high melt strength.
Pellets should be stored in sealed containers below 40 °C and protected from direct sunlight. If stored in an unheated warehouse and moved to a warmer production hall, condensation can raise surface moisture above 0.1 wt%. Pre-drying at 70–80 °C for 2–4 h with a desiccant dryer or hot-air hopper is then required before extrusion. Storage beyond 12 months should trigger re-testing of oxidation induction time and melt mass-flow rate, even if the original certificate of analysis remains within specification. The resin is not intended for rotational molding, thin-wall injection molding, or blown film production. Converting an existing PE80 line to HMCRP100N requires pilot-scale confirmation of melt temperature, head pressure, and hydrostatic burst performance before full production is approved.