| HS Code | 398995 |
| Density | 0.948 g/cm³ |
| Melt Flow Rate | 0.8 g/10 min |
| Tensile Yield Strength | ≥25 MPa |
| Tensile Strength At Break | ≥30 MPa |
| Elongation At Break | ≥600% |
| Flexural Modulus | ≥1000 MPa |
| Notched Izod Impact Strength | ≥20 kJ/m² |
| Vicat Softening Temperature | ≥120 °C |
| Melting Point | 130 °C |
| Hardness | 60 Shore D |
| Environmental Stress Crack Resistance | ≥1000 h |
| Brittleness Temperature | ≤-70 °C |
| Water Absorption | ≤0.01% |
As an accredited Sinopec Qilu HDPE DGDB2480 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinopec Qilu HDPE DGDB2480: packaged in 25 kg PP woven bags, 40 bags per pallet (1000 kg). |
| Container Loading (20′ FCL) | Sinopec Qilu HDPE DGDB2480 loaded in 20′ FCL: 25 kg bags, palletized or loose, approx. 20–25 MT per container. |
| Shipping | Shipping: Sinopec Qilu HDPE DGDB2480 is packed in 25 kg PP woven bags, palletized, shrink-wrapped, and transported in clean, dry containers/trucks. It is non-hazardous; keep dry, away from sunlight and heat. No special IMDG requirements. Store in cool, ventilated warehouse. Avoid moisture, contamination, and sharp objects. |
| Storage | Store Sinopec Qilu HDPE DGDB2480 in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, and ignition sources. Keep original bags or packaging closed and pallets off the floor to prevent moisture and contamination. Avoid contact with strong oxidizers, acids, and bases. Stack securely to prevent deformation, and follow first-in, first-out stock rotation. |
| Shelf Life | Sinopec Qilu HDPE DGDB2480 has a typical shelf life of 24 months when stored cool, dry, and away from direct sunlight. |
Municipal potable water transmission mains extruded from Sinopec Qilu HDPE DGDB2480 operate inside the PE100 pressure window established by ISO 9080:2012 and ISO 12162:2009, where the lower confidence limit of hydrostatic strength is 10 MPa at 50 years and 20 °C. Pipe product conformity to dimensional and pressure-class requirements is audited under ISO 4427-2:2019 and EN 12201-2:2011+A1:2018; potable-contact suitability in North America is tested under NSF/ANSI 61, while AS/NZS 4130:2018 applies in Australasian specifications. A typical converter formulation for black solid-wall pipe consists of 97.5–98.0 wt% DGDB2480 and 2.0–2.5 wt% well-dispersed carbon black masterbatch, with carbon black dispersion verified by ISO 18553 at the pellet or pipe surface. Extrusion is carried out on a high-torque single-screw machine with a grooved feed throat, barrier screw, and 30:1–37:1 L/D; barrel zones are profiled from 180 °C to 220–230 °C, while die head zones are held at 200–220 °C. Melt temperature must not exceed 230 °C; excursions above this threshold accelerate oxidative chain scission and produce visible streaking and reduced hydrostatic strength. Downstream equipment includes vacuum calibration sleeves, multi-chamber spray cooling with water temperatures staged between 20 °C and 40 °C, and planetary or cleat haul-off. Terminal product types are solid-wall pressure pipes in SDR 11, SDR 13.6, SDR 17, and SDR 21, covering PN10 to PN25, with diameters from 20 mm to 2000 mm. When storage humidity exceeds 60% RH, pellets require hopper drying at 80 °C for 1–2 h to remove surface condensation. Mechanical transition couplings are required when the PE100 main is connected to solvent-welded PVC spools, because solvent cements and primers are incompatible with the polyethylene surface.
For fuel gas distribution, the critical material requirement is resistance to rapid crack propagation, and Sinopec Qilu HDPE DGDB2480 is supplied as a PE100 grade qualified against ISO 4437-2:2014 and EN 1555-2; pipe installed in the United States must also conform to ASTM D2513 and the qualification records required under 49 CFR Part 192. RCP performance is measured by the small-scale steady-state S4 test per ISO 13477:2008, with full-scale verification per ISO 13478:2007 where gas utility specifications demand it. Black gas pipe is produced by dosing 2.0–2.5 wt% carbon black masterbatch into the DGDB2480 stream; when yellow line pipe is specified, a coextruded sheath containing 4.0–5.0 wt% cadmium-free yellow masterbatch is applied over a black core that remains DGDB2480-based. The extrusion line typically uses a grooved-barrel single-screw extruder with 33:1 L/D, and screen packs are sized to maintain melt pressure below the extruder's safety limit. Barrel set points increase from 180 °C in the feed zone to 230 °C at the metering zone, with die temperature at 210–220 °C and melt temperature limited to 200–230 °C. The downstream sequence includes vacuum calibration, dual-chamber cooling with water temperatures between 20 °C and 40 °C, ultrasonic wall-thickness measurement, and laser diameter control before cutting or coiling. Terminal products are SDR 11 and SDR 17 gas mains from 20 mm through 630 mm diameter, commonly operated at ≤10 bar for natural gas after applying service-temperature de-rating factors. Operational boundaries include a prohibition on post-consumer recyclate in the pressure wall under most utility specifications; clean in-house regrind may be used only when its melt flow rate remains within the certified range and after drying at 80 °C for 1–2 h.
| Application boundary | Standard designation | Controlling parameter |
|---|---|---|
| Long-term hydrostatic classification | ISO 9080:2012; ISO 12162:2009 | PE100, MRS 10 MPa |
| Potable water pipe conformity | ISO 4427-2:2019; EN 12201-2; NSF/ANSI 61 | Solid-wall PE100, SDR 11–21 |
| Fuel gas pipe conformity | ISO 4437-2:2014; EN 1555-2; ASTM D2513 | ISO 13477 RCP, ≤10 bar MAOP |
| Industrial effluent immersion testing | ISO 15494; ISO 4433-1 | Mass and tensile retention after chemical exposure |
Dredge and mine tailings transport imposes a different set of extrusion constraints on DGDB2480 because the pipes are thick-walled, often SDR 7.4 or SDR 9, and are produced in diameters from 200 mm to 1600 mm. Pressure design references the PE100 long-term strength basis of ISO 9080:2012 and ISO 12162:2009, while product dimensional and pressure testing commonly follows ISO 4427-2:2019 or ASTM F714 depending on the project specification. The formulation is kept close to 97.5–98.0 wt% DGDB2480 with 2.0–2.5 wt% carbon black masterbatch; a fluoropolymer processing aid at 0.05–0.10 wt% is introduced only when melt pressure at constant screw speed rises by more than 10% or when surface die lines appear on thick-wall sections. The principal downstream bottleneck is residual thermal stress caused by inadequate cooling of heavy pipe walls. Extrusion therefore uses a low-output high-torque grooved-barrel single-screw machine with a barrier screw of 30:1–37:1 L/D, barrel temperatures from 180 °C to 220 °C, die temperature 200–220 °C, and a cooling system with long water baths or spray tunnels held at 20–30 °C. Wall-thickness monitoring by ultrasonic transducers and continuous ovality gauging is required to maintain dimensional stability. Terminal products include solid-wall slurry lines, tailings discharge pipes, and dredge floating sections assembled with flanged or butt-fused joints. The material’s chemical resistance is limited in the presence of concentrated oxidizing acids, aromatic hydrocarbon phases, and chlorinated solvents above 40 °C; slurry streams containing these constituents should be evaluated by immersion testing under ISO 4433-1 or ISO 175 before pipe qualification.
Industrial effluents require both pressure integrity and chemically specific compatibility, and DGDB2480 is used in solid-wall chemical drain and effluent trunk lines where intermittent acid or alkali contact is expected. System qualification is conducted under ISO 15494 for industrial plastics piping, and chemical compatibility is established by immersion testing per ISO 4433-1 or ISO 175, with acceptance based on retained tensile elongation and weight change after exposure. The compound formulation for chemical service avoids calcium carbonate fillers and amine-based antistatic masterbatches, because these additives can react or migrate at the pipe surface under low-pH exposure; a standard black formulation uses 97.5–98.0 wt% DGDB2480 and 2.0–2.5 wt% carbon black masterbatch with high-purity furnace black to minimize sulfur and ash contribution. Downstream production is performed on a single-screw extruder with 33:1 L/D and barrel temperatures 180–230 °C, followed by vacuum sizing and controlled cooling to reduce frozen-in stresses. Joining uses butt fusion with oxide removal by rotary planer, bead inspection, and pressure-time profiles per ISO 21307 or national equivalent; electrofusion is permitted when joint surfaces are cleaned and scraped to remove oxidized skin. Terminal products are solid-wall effluent mains in SDR 17 and SDR 21, typically PN10 or PN16, from 50 mm to 1200 mm diameter. The operational boundary is severe: continuous exposure to concentrated nitric acid, strong halogens, or aromatic hydrocarbon solvents above 40 °C is not recommended because these media can initiate environmental stress cracking or oxidative degradation. Published data for this specific resin immersed in mixed solvent matrices is limited; therefore each aggressive stream should be tested under the exact operating temperature and concentration before pipe specification is frozen.
Structured-wall stormwater retention and large-diameter culvert pipe made with DGDB2480 places the high-molecular-weight PE100 resin in the load-bearing layer of a profile-wall or corrugated structure. Product standards include EN 13476-2 for structured-wall non-pressure drainage and sewerage systems, ASTM F2306 for annular corrugated HDPE pipe, and AASHTO M294 for highway drainage applications. In the virgin load-bearing layer, the formulation is maintained at 97.5–98.0 wt% DGDB2480 and 2.0–2.5 wt% carbon black masterbatch; clean in-house regrind from the same production batch may replace up to 15 wt% of the compound only if the melt flow rate and density remain inside the certified windows. The downstream process uses a vacuum corrugator positioned after the die; the melt is formed into annular ribs or a structured wall under vacuum, and cooling water is applied at 20–30 °C to set geometry before cutting. Extrusion parameters are gentler than solid-wall pressure pipe: barrel temperatures are set from 180 °C to 210 °C, die temperatures at 195–210 °C, and melt temperature is held below 220 °C to prevent sag in the unsupported corrugation zone. Terminal product types include stormwater detention/infiltration chambers, culverts, retention tank shells, and cable protection ducts from 100 mm to 3000 mm inside diameter. The material’s high environmental stress crack resistance is leveraged in cyclic stormwater loading, but long-term external load design must be verified through ring stiffness tests under ISO 9969 and creep ratio tests under ISO 9967. Incompatibility with solvent-based jointing compounds remains; structured-wall connections should use elastomeric gaskets or butt fusion for solid-wall sections.
Horizontal directional drilling installations of PE100 water intake and marine outfall lines made from DGDB2480 require both pipe pressure design and pull-force analysis. The governing standards are ISO 4427-2:2019 for the pressure pipe itself, AWWA M55 for PE pipe design and installation, and ASTM F1962 for maximum pulling force calculation under HDD conditions. The pipe formulation is a black solid-wall compound with 2.0–2.5 wt% carbon black masterbatch and 97.5–98.0 wt% DGDB2480; UV stabilization is provided by the carbon black level, and additional additive packages are not required for buried service. Production is performed on a high-output single-screw extruder with 30:1–37:1 L/D, barrel set points 180–230 °C, die 200–220 °C, and vacuum cooling with internal bead control. The downstream process includes butt fusion of pipe strings per ISO 21307, with fusion bead width and alignment checked before pullback; pull force is derived from the bore geometry, drilling mud pressure, and the pipe’s allowable tensile load as calculated under ASTM F1962. Terminal product types are HDD-installed water intake lines, marine outfall pipes, and river crossing force mains, commonly in SDR 11, SDR 13.6, or SDR 17, with diameters from 200 mm to 1600 mm. The main process limitation is fusion joint integrity under sustained pullback; joints must cool to ≤50 °C surface temperature before entering the bore, and pullback speed is limited by bore stability and allowable pull force. No additional backfill material is required beyond the specified annular grout.
Competitive Sinopec Qilu HDPE DGDB2480 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Qilu HDPE DGDB2480 belongs to the producer’s high-density polyethylene pipe-extrusion series, where the grade is specified for extruded pressure conduits rather than high-speed injection moulding. The resin is supplied in pellet form. Published technical bulletins position DGDB2480 as a high-molecular-weight bimodal polyethylene. In a bimodal architecture, the low-molecular-weight fraction controls screw torque and melt flow, while the high-molecular-weight fraction increases the concentration of interlamellar tie molecules. That structural separation has direct consequences for slow crack growth resistance under sustained internal pressure. Table 1 reproduces the property envelope most frequently referenced in producer literature and buyer specifications. The values are representative published ranges and do not replace a certificate of analysis.
| Property | Test method | Published representative value or range |
|---|---|---|
| Density at 23 °C | ISO 1183-1:2019 | 0.947–0.951 g/cm³ |
| Melt mass-flow rate at 190 °C / 5 kg | ISO 1133-1:2022 | 0.20–0.40 g/10 min |
| Tensile stress at yield | ISO 527-2:2012 | 18–23 MPa |
| Tensile elongation at break | ISO 527-2:2012 | >600% |
| Flexural modulus | ISO 178:2019 | 700–900 MPa |
| Environmental stress cracking resistance, F50 | ASTM D1693 condition B | >1000 h |
| Oxidation induction time | ISO 11357-6:2018 | >20 min at 200 °C |
The melt-flow rate condition uses 190 °C and 5 kg because the 2.16 kg condition does not discriminate high-molecular-weight pipe grades. A complete ISO 13479 notched pipe data set is not consistently published in the public bulletin for DGDB2480; where data are absent, the gap is noted rather than supplemented with unverifiable values.
Relative to a unimodal HDPE of similar density, DGDB2480 exhibits a broader molecular weight distribution and a higher concentration of high-molecular-weight chains. The bimodal distribution reduces the tendency for brittle crack propagation by increasing tie molecules between lamellae. This is not a stiffness upgrade; the density and yield stress remain within the PE80 pipe-resin range.
Relative to PE100 resins, the grade is positioned at the PE80 classification level under ISO 12162. The long-term hydrostatic strength lower confidence limit for PE80 is 8.0 MPa at 20 °C and 50 years, whereas PE100 requires 10.0 MPa under the same protocol. The pressure classification translates directly into pipe geometry. For a nominal pressure of 16 bar at 20 °C, a PE80 system with an approximate design stress of 6.3–6.4 MPa requires SDR 9, while a PE100 system at 8.0 MPa requires SDR 11. The PE80 pipe therefore has a thicker wall at equal outside diameter, reducing internal bore and increasing polymer mass per metre. This difference is a design consequence of the MRS classification and not a processing defect.
Compared with injection-moulding HDPE grades of similar density, DGDB2480 has low melt-flow rate and high melt elasticity. Thin-wall injection moulding of fittings is not a recommended use; fill pressure and cycle time exceed normal boundaries for small parts. High-speed extrusion of large-diameter pipe is the target conversion route. The grade is also not interchangeable with general-purpose blow-moulding or film HDPE, because the stabilizer package and molecular architecture are selected for long-term hydrostatic service rather than rapid cycling.
On single-screw pipe extrusion lines with 30:1 to 38:1 L/D grooved-barrel extruders, DGDB2480 is converted at die-entry melt temperatures between 210 °C and 230 °C. The feed zone is normally held at 170–190 °C, and the metering zone is limited to approximately 220 °C. Use of a gear pump between the extruder and die reduces screw-speed-induced surging. For similar bimodal PE80 compounds running 110–250 mm outside-diameter pipe, die-head pressures are frequently observed in the 180–280 bar range; DGDB2480-specific data should be collected for each tooling configuration because published tooling-specific data is limited.
Screen-pack differential pressure is a primary processing boundary. A rise above 80–120 bar across the screen pack indicates gel accumulation, degraded skins, or foreign-particle loading. Melt temperature must not be increased beyond 240 °C to force output. Above that threshold, the hindered phenolic and phosphite stabilizer package is consumed rapidly, and the resulting oxidative damage may not be visible at the die. The failure may appear later as reduced oxidation induction time and shortened service life. If die pressure exceeds equipment-rated limits, output must be reduced rather than increasing barrel temperature. Melt temperature should be measured with an immersion probe at the screw tip and at the die land; a longitudinal difference greater than 10 °C between die quadrants indicates poor thermal homogeneity and may require screw or head revision.
Die swell is greater than that of unimodal HDPE of equivalent melt-flow rate. The die gap is commonly opened 10–20% relative to lower-viscosity grades to maintain final wall thickness. Calibration should control cooling water temperature to avoid residual stress. Thick-wall pipe produced with excessively cold water may retain frozen-in orientation that lowers slow crack growth resistance under ISO 13479 testing.
In buried water supply, ISO 4427-1 and ISO 4427-2 govern polyethylene pipe systems. DGDB2480 is specified as a PE80 base resin for water, raw water, industrial transfer, and drainage rising mains. The long-term hydrostatic strength is validated by ISO 9080 regression analysis. Pressure ratings are temperature-dependent; service at 40 °C requires a derating factor from ISO 4427-1, not an extrapolation of the 20 °C rating.
In mining slurry service, HDPE is selected for abrasion resistance and crack tolerance under rock-fines point loading. However, no standardized abrasion index is published for neat DGDB2480. Abrasion performance must be tested against the specific slurry particle size, velocity, and pH. Published data for this configuration is limited.
Joining is dominated by butt fusion under ISO 21307:2017 and electrofusion under ISO 12176-1. Gas distribution pipe must meet ISO 4437 or the relevant national regulation such as GB 15558.1. Potable water requires separate hygiene certification, including migration testing under the applicable national standard. The base resin designation alone does not confer final pipe-system compliance.
Because slow crack growth is the dominant long-term failure mode in pressurised PE pipe, environmental stress cracking resistance is the most discriminating property. Public summaries for DGDB2480 typically cite ESCR F50 above 1000 h under ASTM D1693 condition B. ASTM D1693 is an indicator test; critical applications should require pipe-specific resistance to slow crack growth via ISO 13479 notched pipe testing.
Slow crack growth initiates at microscopic defects or inclusions. The high-molecular-weight fraction resists craze fibril rupture because tie molecules are stretched across the craze zone; the low-molecular-weight fraction permits processing. This is why a PE80 pipe can exhibit a lower brittle-to-ductile transition stress than PE100 while still outperforming unimodal HDPE in constant-pressure service.
Oxidation induction time measured by ISO 11357-6:2018 at 200 °C is reported above 20 min for stabilised compounds. This value is not a service-life estimate; it signals remaining stabilizer capacity. Storage in direct sunlight or contaminated silos can reduce oxidative stability before extrusion. Blending with post-industrial recyclate of unknown antioxidant history, acidic fillers, or metal-stearate residues is incompatible without separate qualification, because these contaminants can deactivate the stabilizer package. Processing above 240 °C or repeated re-extrusion of regrind shortens long-term hydrostatic strength and should be avoided unless revalidation by ISO 9080 or equivalent is performed.
For outdoor storage, HDPE pellets must be protected from direct ultraviolet exposure. Black pipe compounds achieve UV resistance through carbon black dispersion, typically 2.0–2.5% by mass, evaluated by ISO 18553. The base resin alone is not UV-stabilised. Bags should be kept below 40 °C and away from ground moisture. HDPE is hydrophobic and does not require pre-drying unless surface condensation is present. If condensation occurs, convective drying at 80 °C for 2–4 h is adequate.
Standards compliance for DGDB2480-based pipe compounds is verified by the matrix in Table 2. The matrix separates resin-level tests from finished-pipe system tests. It does not claim that every test is performed on the neat resin; system-level properties are measured on finished pipe or on specimens machined from pipe wall.
| Property or system | Standard designation |
|---|---|
| Density | ISO 1183-1:2019 |
| Melt mass-flow rate | ISO 1133-1:2022 |
| Tensile properties | ISO 527-2:2012 |
| Flexural modulus | ISO 178:2019 |
| Environmental stress cracking resistance | ASTM D1693 condition B; ISO 16770:2019 |
| Notched pipe slow crack growth | ISO 13479 |
| Oxidation induction time | ISO 11357-6:2018 |
| Long-term hydrostatic strength | ISO 9080 |
| Pipe material classification | ISO 12162 |
| Water supply pipe systems | ISO 4427-1, ISO 4427-2 |
| Gas supply pipe systems | ISO 4437 |
| Butt fusion joining | ISO 21307:2017 |
| Electrofusion joining | ISO 12176-1 |
| Carbon black dispersion in black pipe | ISO 18553 |