| HS Code | 690961 |
| Density | 0.949 g/cm³ |
| Melt Flow Rate | 0.08 g/10 min (190°C/2.16 kg) |
| Tensile Yield Strength | ≥24 MPa |
| Elongation At Break | ≥600% |
| Flexural Modulus | ≥1000 MPa |
| Vicat Softening Point | ≥125 °C |
| Brittleness Temperature | ≤-70 °C |
| Environmental Stress Crack Resistance | ≥1000 h |
| Notched Izod Impact Strength | ≥40 kJ/m² |
| Hardness | ≥60 Shore D |
| Melting Point | 130 °C |
| Water Absorption | <0.01% |
| Dielectric Constant | 2.3 |
| Volume Resistivity | >10^16 Ω·cm |
| Dielectric Strength | ≥20 kV/mm |
| Thermal Conductivity | 0.45 W/m·K |
| Coefficient Of Linear Thermal Expansion | 1.2×10^-4 /°C |
As an accredited Sinopec Qilu HDPE DGDA6098 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinopec Qilu HDPE DGDA6098 is typically packaged in 25 kg PP woven bags with PE inner liners for safe transport. |
| Container Loading (20′ FCL) | 20′ FCL loaded with 25 MT Sinopec Qilu HDPE DGDA6098 in 25 kg bags, securely stowed and wrapped for export. |
| Shipping | Sinopec Qilu HDPE DGDA6098 is a non-hazardous thermoplastic resin, shipped as pellets in 25 kg bags or 1,000 kg jumbo bags, palletized and shrink-wrapped. It moves by standard sea or land freight in clean, dry containers. Protect from moisture, heat, and direct sunlight. No dangerous goods handling required. |
| Storage | Store Sinopec Qilu HDPE DGDA6098 in a cool, dry, well-ventilated warehouse, away from direct sunlight, rain, and moisture. Keep original bags or containers closed to prevent contamination. Avoid heat, flames, sparks, and strong oxidizers. Use first-in, first-out stock rotation. Stack pallets securely to prevent bag damage. Keep area clean and free from dust and incompatible materials. Maintain ambient storage temperature. |
| Shelf Life | Shelf life is typically 24 months when stored in original packaging, in a cool, dry, ventilated area, away from sunlight and moisture. |
For T-shirt carrier bag conversion lines, Sinopec Qilu DGDA6098 is processed as a high-molecular-weight HDPE blown film resin on single-screw extruders with L/D 24:1–30:1, barrier screws incorporating a Maddock mixing section, and die diameters between 80–120 mm. Melt temperature is maintained at 200–220°C, with die lip temperature controlled at 190–210°C and die gap set between 1.2–1.8 mm. Blow-up ratio is typically 4:1–6:1, producing film gauge in the 12–35 µm range. Formulation addition ratios for this segment commonly include 10–20 wt% LLDPE to raise dart impact strength and tear propagation, 2–4 wt% color masterbatch, and 1–2 wt% slip/antiblock masterbatch or active slip loadings of 500–1500 ppm. Compliance evaluation for finished retail bags follows EU Directive 94/62/EC packaging heavy metal limits requiring total lead, cadmium, mercury, and hexavalent chromium content not exceeding 100 ppm; mechanical testing is performed under ISO 527-3:2018 for tensile properties and ISO 7765-1:1988 for dart impact. Downstream conversion includes corona treatment to 38–42 dyn/cm for flexographic print adhesion, followed by in-line bag conversion. Operational boundaries include die lip build-up at elevated output and bubble instability when frost-line height exceeds 8–12 times die diameter. Terminal product types include T-shirt carrier bags, produce roll bags, and small boutique bags.
For monolayer heavy-duty sack extrusion, gauge uniformity is governed primarily by bubble cooling stability and frost-line control rather than extruder throughput alone. On production lines running Sinopec Qilu DGDA6098 at film thicknesses of 60–120 µm, die gap is widened to 1.5–2.0 mm and blow-up ratio is reduced to 3:1–4:1 to limit transverse gauge variation. Frost-line height is held at 8–12 times die diameter to stabilize the high-molecular-weight HDPE bubble; deviation from this window produces edge wrinkling and uneven roll hardness. Formulation addition ratios for industrial sack grades include 20–30 wt% LLDPE or 10–20 wt% metallocene LLDPE for tear improvement, 3–6 wt% carbon black masterbatch for UV resistance in outdoor storage, and 300–800 ppm antioxidant. Compliance testing is anchored to ASTM D1709-16a for dart drop, ISO 6383-2:1983 for trouser tear, and ISO 527-3:2018 for tensile strength and elongation at break. Downstream production equipment includes high-stalk blown film lines with dual-lip air rings, gusseting stations, and rotary die heads; film roll widths commonly range from 400–1200 mm. Failure modes observed on industrial lines include melt fracture at high screw speed, fold crease splitting when film gauge drops below 60 µm, and carbon black dispersion defects when masterbatch is added without adequate distributive mixing. Terminal product types include construction rubble bags, insulation packaging sacks, and heavy-duty industrial refuse sacks.
Post-consumer recycled HDPE introduces viscosity heterogeneity, volatile carryover, and gel-particle contamination that alter the processing boundary for DGDA6098 in institutional waste bag production. Extruders are typically configured with vented barrels or PCR is pre-dried at 70–80°C for 2–4 h when ambient relative humidity exceeds 60%. Melt temperatures are limited to 190–210°C to avoid off-gassing and localized oxidation. Formulation addition ratios in this segment generally include 20–40 wt% PCR HDPE blended into DGDA6098, with 10–20 wt% LLDPE added to restore dart impact and reduce splitting at seal junctions. Screen packs of 120/150 mesh are required upstream of the die to capture gel particles and paper label residues. Compliance evaluation follows EN 13592:2017 for household waste collection sacks and REACH 1907/2006 Article 33 obligations for SVHC communication in recycled feedstock. Mechanical test methods include ISO 7765-1:1988 for dart impact and ASTM D1922-15 for Elmendorf tear. Downstream production uses blown film lines with internal bubble stabilization and thickness gauges calibrated for 30–80 µm film. Operational boundaries include reduced bubble stability at PCR addition above 40 wt% and seal-strength loss when recycled content introduces crosslinked particles. Terminal product types include hospital waste bin liners, commercial refuse sacks, and institutional black refuse bags.
In a three-layer coextrusion line, DGDA6098 functions as the HDPE core layer in dry food packaging films where moisture barrier and stiffness are primary requirements. The core layer addition ratio is normally 40–60 wt% of the total film structure, with LDPE or LLDPE skins forming the remaining 20–35 wt% per layer depending on sealant performance and coefficient of friction targets. Total film gauge is typically 20–50 µm, die gap is held at 1.2–1.8 mm, and blow-up ratio is set at 3:1–4:1. Slip and antiblock additives are confined to the skin layers, while the HDPE core remains unmodified to preserve barrier integrity. Compliance for direct food contact is assessed under FDA 21 CFR 177.1520 for olefin polymers, EU Regulation 10/2011 with overall migration limits of 10 mg/dm², and GB 4806.7-2016 for China food-contact plastic materials and articles. Downstream conversion includes three-layer blown film extrusion with gravimetric dosing, corona treatment to 38–42 dyn/cm, and lamination or printing before pouch forming. Failure modes observed on food packaging lines include interfacial flow instability when skin and core melt viscosities diverge excessively, migration of slip agents into the core at high processing temperatures, and odor carryover from PCR-free but lightly oxidized core material. Terminal product types include cereal liners, cracker bags, dry mix pouches, and snack packaging inner webs.
For chemical powder drum liners and flexible intermediate bulk container inner liners, seal integrity and moisture transmission are more critical than print appearance. Formulation is commonly 100 wt% virgin DGDA6098 or a blend containing 10–20 wt% metallocene LLDPE for low-temperature seal strength. Antistatic masterbatch is added at 0.2–1.0 wt% only when required for powders with high dust explosion potential, and the addition must be evaluated for compatibility with chemical contact. Film gauge is maintained between 50–100 µm, die gap is set at 1.5–2.0 mm, and blow-up ratio is constrained to 2.5:1–3.5:1 to maximize bubble stability with filled or viscous formulations. Heat sealing temperatures are typically 130–150°C with dwell times adjusted to achieve hermetic seams. Compliance evaluation follows UN Model Regulations Chapter 6.1 for packaging compatibility in dangerous goods transport, ISO 7765-1:1988 for puncture and dart resistance, and ASTM D882-18 for thin-film tensile properties. Downstream production routes include blown film extrusion, in-line slitting, and conversion into pre-sealed liners with tear-off closures. Operational boundaries include dust contamination at seal areas, pinhole formation when film gauge drops below 50 µm, and stress cracking in contact with aggressive surfactants; published data for DGDA6098-specific chemical resistance in aggressive solvent contact is limited. Terminal product types include drum liners, FIBC inner liners, box liners, and powder transfer sleeves.
Coextruded poly mailers using DGDA6098 as a stiff skin layer require precise skin-to-core ratio control to balance tear resistance, puncture resistance, and flexographic print adhesion. In a three-layer structure, the HDPE skin layer addition ratio is 15–25 wt% of total film mass, with an LDPE or LLDPE core comprising 70–80 wt% and white masterbatch added at 2–5 wt% in the core or skin. Total film thickness ranges from 50–100 µm, die gap is set at 1.4–1.8 mm, and blow-up ratio is typically 3:1 to preserve bubble symmetry. Surface treatment to 40–44 dyn/cm is required before flexographic ink application; untreated HDPE surfaces below 38 dyn/cm produce inconsistent ink transfer and abrasion failure. Mechanical compliance is verified under ISO 527-3:2018 and ASTM D882-18, while packaging heavy metal restrictions follow EU Directive 94/62/EC. Downstream conversion includes three-layer blown film extrusion, surface corona treatment, flexographic printing, and automated bag fabrication with self-adhesive closures. Failure modes on mailer lines include layer delamination when skin-to-core melt viscosity ratio exceeds processing limits, fisheye formation from oxidized HDPE gels, and ink smearing when corona treatment decays below 40 dyn/cm in high-humidity storage. Terminal product types include e-commerce poly mailers, courier envelopes, and opaque shipping bags.
Thick HDPE sheeting produced from DGDA6098 for temporary construction vapor retarders and containment applications is processed with a wider die gap to offset high melt viscosity at increased gauge. Film thickness in this segment is typically 100–200 µm, requiring die gap settings of 1.8–2.5 mm and blow-up ratios of 2.5:1–4:1. Formulation addition ratios include 2–4 wt% UV stabilizer masterbatch for outdoor exposure and 2–4 wt% carbon black masterbatch when opacity and long-term weathering are specified. Melt temperature is held at 190–210°C to limit gel generation during extended run periods. Water vapor transmission testing is conducted under ASTM E96/E96M-22a; sheeting for below-slab vapor retarder duty is commonly evaluated against ASTM E1745-17 for puncture and tensile requirements. Downstream production uses slow-cooled blown film towers with gauge scanners and surface winders configured for wide rolls. Field experience indicates that edge cracking occurs when winding tension exceeds film yield limits at thicknesses below 100 µm, and bubble instability increases when blow-up ratio exceeds 4:1 at low melt stiffness. Published product-specific data for DGDA6098 in vapor retarder service remains limited, so conversion parameters are generally derived from comparable high-molecular-weight HDPE film grades. Terminal product types include temporary construction vapor retarders, concrete curing sheeting, containment sheeting, and surface protection films.
Competitive Sinopec Qilu HDPE DGDA6098 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Qilu HDPE DGDA6098 is a high-density polyethylene film extrusion resin supplied in pellet form. The producer’s technical datasheet identifies the grade by a nominal density of 0.949 g/cm³ and a melt mass-flow rate at 190 °C under 2.16 kg load of 0.08 g/10 min when measured to ISO 1133-1:2022. The product is specified for heavy-duty sacks, industrial liners, carrier bags, and multi-wall packaging structures in which film gauge is reduced without a corresponding loss of puncture resistance. Because the resin has a low melt index, extrusion requires higher head pressure and more controlled melt-temperature management than is typical for high-melt-index HDPE film grades. Table 1 lists producer-published typical values; these are not to be read as guaranteed specification limits for every production lot.
| Property | Test method | Typical value |
|---|---|---|
| Melt mass-flow rate, 190 °C/2.16 kg | ISO 1133-1:2022 | 0.08 g/10 min |
| Density at 23 °C | ISO 1183-1:2019 | 0.949 g/cm³ |
| Tensile stress at yield, machine direction | ISO 527-3:2018 | 25 MPa |
| Elongation at break, machine direction | ISO 527-3:2018 | 600 % |
| Dart drop impact, F50 | ASTM D1709A | 300 g |
| Vicat softening temperature | ISO 306/A50 | 124 °C |
The combination of a density of 0.949 g/cm³ with a low melt mass-flow rate places DGDA6098 in the high-molecular-weight, high-density polyethylene film segment. The density provides lower water-vapour transmission than an LLDPE grade with a density of 0.920 g/cm³ when films of equal gauge are compared under ISO 15106-3 conditions, although the final barrier depends on film structure and orientation. The low melt index is the dominant variable for bubble stability and head-pressure generation in downstream conversion.
The principal difference is rheological. The melt index of 0.08 g/10 min at 190 °C under 2.16 kg corresponds to a higher average molecular weight than conventional HDPE film grades with I₂ values of 0.7–1.2 g/10 min. Higher molecular weight increases zero-shear viscosity and elongational viscosity, which supports bubble stability under blow-up ratios of 2.5:1–4.0:1 and long-stalk drawing. The trade-off is increased melt resistance. On a 90 mm single-screw extruder with 30:1 L/D, DGDA6098 is observed to generate 15–25 % higher head pressure than an I₂ 1.0 g/10 min HDPE film resin at the same screw speed and die geometry. This difference requires screw designs with adequate torque and screen-pack area; otherwise melt temperature can rise above the 230 °C degradation threshold.
In blown-film conversion, the low melt index also influences molecular orientation. Because high-molecular-weight chains relax more slowly after leaving the die, a frost line height set too low freezes orientation in the machine direction and produces films with reduced tear resistance in that direction. The balance between machine-direction and transverse-direction properties is therefore adjusted by blow-up ratio and frost line position, not by raising melt temperature alone. This behaviour differs from high-melt-index HDPE grades, which relax faster and require shorter frost line distances but show lower melt strength.
The resin is processed on single-screw extruders with L/D ratios not lower than 25:1, preferably 30:1. Barrel temperature settings are typically: feed zone 40–60 °C, compression zone 180–195 °C, metering zone 200–210 °C, and die zones 205–220 °C. The recommended melt temperature is 200–225 °C; below 195 °C, sharkskin melt fracture may appear on the inner bubble surface, while sustained operation above 230 °C accelerates oxidative chain scission and reduces Elmendorf tear after film ageing. The die gap is kept between 1.6 mm and 2.4 mm, with a blow-up ratio of 2.5:1–4.0:1. For a 300 mm die diameter, the frost line height is often set at 2,400–3,000 mm, equivalent to eight to ten die diameters. This setting stabilizes the bubble and balances machine-direction and transverse-direction properties.
Internal bubble cooling is used when output exceeds 180–200 kg/h; without IBC, bubble sag and gauge variation may exceed ±8 %. Screen packs of 100/120 mesh are installed to increase homogenization pressure, with pressure drop across the screen pack reaching 35–45 bar at normal output. The melt pressure requirement should be considered when selecting the extruder drive and screw cooling system. Screen-pack blockage can become a processing bottleneck if recycled scrap contains paper or metal fines; the resulting pressure rise reduces output and raises gel formation.
Pellets that have been cold-stored below -10 °C and transferred to a humid processing bay may develop surface condensation. If ambient relative humidity exceeds 80 %, a hopper dryer at 60–70 °C for 2–3 h is used before extrusion to avoid surface voids and melt-phase moisture bubbles. Resin stored in sealed containers at ambient temperature normally does not require drying.
In industrial liner and carrier bag production, DGDA6098 is often placed as the core layer in three-layer coextrusion with LLDPE skins. The LLDPE skins contribute low-temperature impact, while the DGDA6098 core contributes modulus and melt strength. This layer structure permits down-gauging to 50–70 µm while maintaining drop and puncture performance. At this gauge, dart drop resistance is measured to ASTM D1709A, and Elmendorf tear is measured to ISO 6383-2:2020. The use of a core layer also allows recycled edge trim to be reintroduced without direct contact with the film surface.
In multi-wall paper lamination, DGDA6098 is processed at a lower melt temperature than LDPE to reduce paper scorching. Melt temperature is maintained at 200–220 °C, and coating thickness is set between 15 µm and 25 µm. The high melt strength reduces neck-in; at a 200 mm die width, neck-in is held below 15 mm at line speeds up to 150 m/min. Published data for this specific configuration is limited.
When film gauge is reduced from 80 µm to 60 µm, a high-melt-index HDPE film often shows a disproportionate reduction in dart impact and Elmendorf tear because crack propagation is constrained by the low-molecular-weight fraction in the film. DGDA6098 retains higher dart impact at equivalent gauge because its lower melt index reflects fewer short-chain molecules and higher entanglement density after solidification. The effect is not linear: below 40 µm, bubble instability and gauge variation, rather than resin molecular weight, usually control failure. The grade is therefore specified for heavy-duty sacks carrying 25–50 kg of free-flowing solids and for industrial liners exposed to sharp protrusions. Acceptance testing in these applications commonly uses ASTM D1709A for dart drop and ISO 6383-2:2020 for Elmendorf tear.
At the same gauge, DGDA6098 films show higher modulus than LLDPE-rich formulations; this permits conversion lines to operate with reduced tensile elongation and improved bag-top stiffness. However, the resin should not be blended with high-MI HDPE scrap above approximately 20 wt% in the core layer. Each increment of high-MI material lowers bubble stability and reduces dart impact at a rate that is not linear. Published data for this specific configuration is limited; the 20 wt% boundary is a production-scale operating guideline rather than a specification limit.
After the bubble is collapsed and trimmed, the film continues to crystallize at a rate set by cooling-air temperature, take-off speed, and film thickness. If the film enters the nip rolls above 70 °C, blocking can occur and subsequent slitting may generate edge tears. On high-speed lines, chill-roll temperature is kept below 50 °C. Rapid cooling from the melt to solid state produces smaller spherulites and generally improves dart impact relative to slow cooling, but rapid cooling also lowers thermal shrinkage resistance unless the film is annealed. For DGDA6098, the high molecular weight tail increases tie-chain density after solidification; this is the structural basis for its higher Elmendorf tear relative to high-MI HDPE at a given density. Property development is measured at 24 h after extrusion because HDPE crystallinity and film dimensions evolve during the first day of storage. Tensile tests run immediately after production may understate elongation to break by up to 10 % relative to the 24 h value.
Antiblock concentrates are used at 2–3 wt% in thin bag film to prevent blocking. Above 5 wt%, dart impact falls because mineral particles initiate crack propagation. Slip-agent masterbatch addition of 500–1,000 ppm erucamide reduces surface friction; the exact level depends on the film structure and final use. The grade is not internally lubricated; all surface properties are controlled by external additives.
For outdoor liners and agricultural film, carbon black masterbatch at 2–3 wt% is used to achieve weathering resistance. Dispersion of carbon black is evaluated under ISO 18553, and poor dispersion lowers dart impact and creates pinholes. Natural grades are recommended for indoor packaging only unless a UV stabilizer system is incorporated by the converter.
Relative to LLDPE film with an I₂ of 1.0 g/10 min and density of 0.920 g/cm³, DGDA6098 yields higher modulus and lower water-vapour transmission but lower low-temperature dart impact. The choice of the resin is therefore made when stiffness, creep resistance, and melt strength control the application. Compared with a generic high-MI HDPE film resin with I₂ of 0.8 g/10 min, the lower melt index of DGDA6098 provides greater bubble stability and thin-gauge impact retention but imposes higher extruder head pressure. Bimodal HDPE film grades may approach the impact performance of DGDA6098 with improved bubble stability under high-speed extrusion, but their regional availability and resin cost may differ.
In recycling streams, DGDA6098 retains its density-based float-sink separability because HDPE with density of 0.949 g/cm³ remains in the olefin float fraction under ISO 1183-1 test conditions. This allows post-industrial trim to be reclaimed and re-extruded in the core layer. Reclaimed film should not exceed 20 wt% of the total composition unless its melt index and density are verified at incoming inspection.
Food-contact compliance declarations are available from the producer under FDA 21 CFR 177.1520 for olefin polymers and GB 9685-2016 where applicable. Final food-contact suitability must be confirmed on the finished structure, because printing inks, adhesives, and outer layers may alter migration behaviour. The resin should not be used in direct contact with strong oxidizing media without prior compatibility testing.