| HS Code | 585529 |
| Density | 0.958 g/cm³ |
| Melt Flow Rate | 0.23 g/10 min (190°C/5 kg) |
| Tensile Strength At Yield | ≥25 MPa |
| Elongation At Break | ≥600% |
| Flexural Modulus | ≥1000 MPa |
| Vicat Softening Point | ≥125°C |
| Brittleness Temperature | ≤-60°C |
| Environmental Stress Cracking Resistance | ≥1000 h |
| Oxidation Induction Time | ≥20 min |
| Carbon Black Content | 2.0-2.5% |
| Hardness | 60-65 Shore D |
| Water Absorption | <0.01% |
| Thermal Conductivity | 0.40 W/(m·K) |
| Coefficient Of Linear Thermal Expansion | 1.2-1.8 × 10⁻⁴ /°C |
As an accredited Sinopec Maoming HDPE TR571M factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinopec Maoming HDPE TR571M typically comes in 25 kg woven bags, palletized and wrapped for industrial shipment. |
| Container Loading (20′ FCL) | Container loading: Sinopec Maoming HDPE TR571M in 20′ FCL, 25kg PP bags, palletized, shrink-wrapped, secured for sea shipment. |
| Shipping | Sinopec Maoming HDPE TR571M is shipped as non-hazardous polyethylene pellets, typically in 25 kg PP/PE bags or 1,500 kg jumbo bags, palletized and stretch-wrapped. Transport in clean, dry, covered containers or trucks, protected from moisture, direct sunlight, heat, and incompatible materials. Standard general cargo; no special IMDG/ADR requirements. |
| Storage | Sinopec Maoming HDPE TR571M should be stored in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, flames, and strong oxidizers. Keep original bags sealed and palletized; avoid moisture, contamination, and excessive stacking pressure. Maintain ambient temperature, preferably below 50°C. Use clean handling equipment. Do not expose to UV radiation or ignition sources. Rotate stock first-in-first-out and follow local regulations. |
| Shelf Life | Shelf life: 24 months from date of manufacture when stored in a cool, dry, ventilated area in unopened original packaging. |
Municipal potable water mains produced from PE100 high-density polyethylene require the resin to meet the long-term hydrostatic strength classification of 10.0 MPa minimum required strength at 20 °C for 50 years under ISO 9080 and ISO 12162. The governing product standards are ISO 4427-2:2019, EN 12201-1:2011, EN 12201-2:2011, GB/T 13663.2-2018, and AS/NZS 4130:2018; where potable-water contact is specified, NSF/ANSI/CAN 61 applies. Sinopec Maoming HDPE TR571M is used in this segment as a PE100 pressure-pipe grade; the lot certificate must confirm the exact MFR5 under ISO 1133-1:2022 and the carbon black content of the compounded pipe material. For natural resin formulations, a 40 wt% carbon black masterbatch is let down at 5.0–6.25 wt% to achieve a final black concentration of 2.0–2.5 wt%; for pre-compounded black variants, the final carbon black concentration remains the same compliance requirement under EN 12201-1. No calcium carbonate, talc, or other mineral filler is added, because inert particles act as stress risers that reduce slow crack growth resistance under hoop stress.
| Pipe OD range | Extruder L/D | Die melt temperature | Cooling water inlet | Closed-loop ultrasonic tolerance |
|---|---|---|---|---|
| DN 110–250 mm | 30–36 | 195–215 °C | 15–25 °C | ±0.1–0.2 mm |
| DN 315–630 mm | 33–38 | 200–225 °C | 15–20 °C | ±0.2–0.3 mm |
| DN 710–1200 mm | 36–40 | 205–225 °C | 10–18 °C | ±0.3–0.5 mm |
On production-scale lines processing DN 315–630 mm pipe, the extruder is typically a 75–90 mm grooved-feed single-screw unit with L/D 33–38, a spiral-mandrel die, and a die-entry melt temperature of 200–225 °C. Die-head pressure is maintained between 18 MPa and 30 MPa; higher pressure loss may indicate carbon black agglomeration or screen-pack blinding after long runs, requiring screen changes at intervals of 4–8 weeks depending on masterbatch quality. The feed-zone temperature is kept below 80 °C to prevent premature melting and bridging in the grooved bushing. Vacuum calibration and spray cooling use water at 15–25 °C; for thick-wall SDR 11 pipe, the cooling gradient is stepped to reduce residual hoop stress. Downstream ultrasonic wall-thickness scanning and a laser diameter gauge provide closed-loop haul-off control. The terminal product range spans DN 110–1600 mm, with SDR 11, 17, or 21 covering nominal pressures from 10 bar to 25 bar. For chlorine dioxide or other oxidative disinfectants, the design pressure must be de-rated in accordance with the pipe manufacturer’s technical guidance and ISO/TR 10358-1, because oxidative degradation accelerates slow crack growth at elevated temperatures.
In buried natural gas distribution networks, the co-extruded yellow identification stripe is not decorative; it is covered by ISO 4437-2:2024, EN 1555-2:2021, GB 15558.1-2023, and ASTM D2513-20. The main black layer carries a final carbon black content of 2.0–2.5 wt%, while the yellow stripe is produced from a cadmium-free organic yellow masterbatch typically added at 2–4 wt% into the outer layer of the co-extruded pipe. The stripe let-down is set by die-land residence time and melt-viscosity mismatch; below 2 wt% pigment masterbatch, the stripe can delaminate from the black substrate at the pipe surface because the melt elongational viscosity differential exceeds 15%, while above 4 wt%, sharkskin may appear at the stripe edges. The terminal gas pipe product range for PE100 grade resin is commonly DN 25–630 mm, SDR 11 or 17, with maximum operating pressure 4–10 bar depending on the gas network class and design factor.
Rapid crack propagation is the controlling failure mode for gas pipe above DN 250 mm at low ambient temperatures. Full-scale RCP tests may be ordered under ISO 13477 using a pipe temperature of 0 °C or lower; on production lines, processors minimize RCP susceptibility by avoiding melt temperatures above 230 °C, because thermo-oxidative chain scission shortens the high-molecular-weight tail that governs slow crack growth resistance. Field experience on extruders with L/D 33–37 shows that batch-to-batch MFR drift of ±0.03 g/10 min can change wall-thickness control by 0.5–1.0 mm at fixed haul-off speed if closed-loop ultrasonic gauging is not applied. Co-extrusion tooling with a spiral mandrel die and three heaters per stripe channel is standard; downstream laser diameter gauges are placed after the first cooling basin to catch stripe geometry deviation before the pipe enters the haul-off.
Chemical-resistance classification, rather than potable-water certification, governs industrial process water and acid-alkali effluent pipe systems based on TR571M. Dimensional and material compliance is established under ISO 15494-1:2015 and ISO 15494-2:2015, while chemical resistance is assessed by ISO/TR 10358-1. For black industrial pipes, the carbon black level remains 2.0–2.5 wt%; if a white or natural pipe is specified for indoor chemical drainage, carbon black is omitted and the stabilizer package is limited to 0.2–0.5 wt% of hindered phenol/phosphite antioxidant masterbatch. The use of calcium carbonate filler is prohibited above 0.5 wt% in acidic effluent service because carbonate leaching creates surface pits that reduce chemical resistance. Thick-wall industrial pipe extrusion uses a slow cooling protocol; wall thickness above 60 mm requires multiple water baths with stepped temperatures of 40 °C, 30 °C, and 20 °C to limit residual hoop stress. The pipe is joined by butt fusion using ISO 21307 procedures. Terminal products are DN 90–1200 mm, SDR 13.6–33, PN 6–16 bar industrial effluent, process water, and acid/alkali transfer lines. Continuous service above 40 °C or with strong oxidizing acids requires chemical-resistance verification and pressure de-rating.
In mineral slurry and tailings transport, the absence of mineral filler in TR571M pipe formulations is deliberate because inert particles reduce slow crack growth resistance under cyclic pressure surges. Dimensional standards for the pipe body are ISO 4427-2:2019 and ASTM F714-24, while installation and joining follow ISO 21307:2017; abrasion performance is normally qualified by project-specific slurry test protocols because no single ISO abrasion standard covers all tailings compositions. The final carbon black content remains 2.0–2.5 wt%, with base resin content above 97 wt%; a 50 wt% carbon black masterbatch is added at 4.0–5.0 wt%, or a 40 wt% masterbatch at 5.0–6.25 wt%. No silica, barium sulfate, or glass-fiber reinforcement is used.
Extrusion of mining-grade solid-wall pipe favors lower line speeds and stepped cooling. For SDR 11 pipe above DN 500 mm, wall thickness can exceed 40 mm, and standard single-stage vacuum calibration becomes insufficient to remove residual stress; multi-stage spray cooling with water at 40 °C, 30 °C, and 20 °C is required. A field observation on high-solids tailings lines is that elbow wear can occur at 3–5 times the straight-pipe wall loss rate, so elbows are either protected with replaceable wear pads or specified at a thicker SDR. The terminal product range for this segment is DN 160–1000 mm, SDR 11–26, pressure ratings 10–25 bar, used for mineral slurry, tailings, and dredge discharge. Ultrasonic wall-thickness checks at bends every 6–12 months are standard practice to maintain leak-before-break performance.
Submerged outfall lines for desalination brine, power-station cooling water, and wastewater discharge use elongated strings of black PE100 pipe that must be dimensionally stable during ballasting, launching, and tow. The governing dimensional and material standards are ISO 4427-2:2019, EN 12201-2:2011, and ASTM F714-24; marine-specific design is typically verified against project specifications rather than a single ISO marine standard. The black compound is formulated to 2.0–2.5 wt% carbon black; above the splash zone, an additional hindered amine light stabilizer package of 0.2–0.5 wt% may be incorporated into the masterbatch, though carbon black remains the primary UV absorber. The terminal product range for marine outfall/intake lines is commonly DN 500–2000 mm, SDR 17 or 21, installed in water depths up to 50 m depending on wall-thickness and collapse resistance.
Fabrication involves shop butt-fusion of pipe sections into strings of 500–2000 m, followed by bolted ballast weights and end bulkheads. In humid coastal conditions, the butt-fusion heating plate must be cleaned every 10–15 joints to remove oxide and salt deposition; otherwise, joint contamination lowers tensile elongation at the fusion interface. Tow-force calculations are based on string weight, buoyancy, and current drag; on large installations, a 1.5–2.0 safety factor over predicted tow stress is required. The minimum bending radius during launching and submergence is controlled by SDR and water temperature; for SDR 17 at 20 °C, the minimum radius is normally not less than 20–25 times the outside diameter.
Before a borehole is drilled for a trenchless carrier pipe, the installed PE100 string must simultaneously resist hoop stress, axial pull stress, and external annular pressure. The drill-path design standard is ASTM F1962-22, with pipe dimensions according to ISO 4427-2:2019 or ASTM F714-24. For HDD strings, the formulation allows up to 10 wt% clean in-house regrind from the same TR571M production line; post-consumer recycled material is excluded because it cannot guarantee slow crack growth resistance. The final carbon black content must remain at 2.0–2.5 wt%, and regrind addition above 10 wt% can reduce the slow crack growth resistance at butt-fusion joints and increase the risk of brittle pull failure.
Pipe strings for HDD are butt-fused in line with ISO 21307; after fusion, the string is pulled through a borehole that is typically 1.3–1.5 times the outside diameter of the pipe. The allowable pull force is computed in ASTM F1962-22 using pipe weight, borehole curvature, drilling-fluid pressure, and buoyancy; the tensile stress during pullback must remain below the safe pull stress published for the pipe, and on-site load cells are placed at the pull head to prevent joint overload. The terminal product is an DN 250–1200 mm, SDR 11 or 17 PE100 pressure pipe installed as a trenchless carrier for water, gas, or conduit. Residual stress from uneven cooling can cause the pipe to kink in the borehole, so processors must maintain stepped cooling and document wall-thickness variance before the string is accepted for pull-in.
Competitive Sinopec Maoming HDPE TR571M prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Maoming HDPE TR571M is a bimodal high-density polyethylene grade supplied as natural pellets for pressure pipe and industrial conduit extrusion. The producer’s published typical values include a melt flow rate of 0.22 g/10 min at 190 °C under 5 kg load per ISO 1133-1:2022, and a density of 0.950 g/cm³ at 23 °C per ISO 1183-1:2019. The bimodal molecular weight distribution separates the high-molecular-weight fraction that governs slow crack growth resistance from the lower-molecular-weight fraction that improves melt extensibility and extruder throughput. This architecture shifts the conventional stiffness-versus-toughness balance compared with unimodal HDPE. Commercial lots are normally controlled within ±0.003 g/cm³ for density and ±0.03 g/10 min for melt flow rate; the certificate of analysis for each lot remains the governing document, not the illustrative typical values.
Published typical property envelope for Sinopec Maoming HDPE TR571M:
| Property | Test method | Typical value |
|---|---|---|
| Melt flow rate at 190 °C/5 kg | ISO 1133-1:2022 | 0.22 g/10 min |
| Density at 23 °C | ISO 1183-1:2019 | 0.950 g/cm³ |
| Tensile stress at yield, 50 mm/min | ISO 527-2:2012 | 23 MPa |
| Nominal tensile strain at break | ISO 527-2:2012 | >600% |
| Flexural modulus | ISO 178:2019 | 850 MPa |
| Charpy notched impact at -30 °C | ISO 179-1:2010 | 12 kJ/m² |
| Oxidation induction time at 200 °C | ISO 11357-6:2018 | >20 min |
| Environmental stress crack resistance, F50 | ASTM D1693-15e1 | >1,000 h |
On a grooved-feed single-screw extruder with L/D 33:1 and screw diameter between 45 mm and 120 mm, TR571M is usually processed with a reverse temperature profile from 190 °C in the feed zone to 215 °C at the adapter and 210 °C at the die. Melt temperatures above 240 °C accelerate thermo-oxidative degradation and shorten hydrostatic failure time; sustained operation below 180 °C increases melt fracture, head pressure, and die-lip deposit formation. The grooved feed bushing is maintained at 40–70 °C to preserve solid conveying; bushing temperatures above 80 °C reduce specific throughput and raise energy consumption. Virgin pellets do not require pre-drying when free moisture is below 0.05 wt%; regrind or silo condensation is handled by dry-air purge at 70–80 °C for 2 h.
Capillary rheometry at 190 °C under ISO 11443:2021 shows pronounced shear thinning; a shear-rate increase from 100 s⁻¹ to 1,000 s⁻¹ can reduce apparent viscosity by 50–70%, which allows high die throughput while retaining high melt strength in the sizing sleeve. The critical shear rate for melt fracture at 190 °C is generally above 500 s⁻¹ for this molecular weight class. Extruders without grooved feed sections may require a slightly higher compression ratio of 3.0:1 to 3.5:1 and a barrier screw to avoid surging.
Startup failure modes on commercial pipe lines often include die-lip melt fracture and charred gel formation. Gels appear when material stagnates in the die head or when the screen pack is not fully packed; pipe pinholes from gel particles reduce burst pressure and require extruder shutdown. Frequent purge with a lower-viscosity HDPE or a purging compound after grade transitions reduces this defect. Batch-to-batch viscosity drift is detected by monitoring melt pressure at constant screw speed; a pressure deviation greater than 10 bar from the reference lot may require a barrel temperature adjustment of 5 °C to retain dimensional stability.
In buried pressure service, the controlling failure mode is usually slow crack growth from scratches, inclusions, or point loading by stones. Pipe made from TR571M is tested under ISO 1167-1:2006 at 20 °C and 80 °C; for PE100 classification, a typical 110 mm SDR 11 pipe must survive hoop stress of 12.4 MPa at 20 °C for 100 h and 10.0 MPa at 80 °C for 165 h. Notched pipe testing under ISO 13479:2009 at 80 °C and 4.0–4.6 MPa is used as a discriminator for brittle failure; bimodal materials of this class typically exceed 500 h when pipe processing is within specification. The high-molecular-weight fraction increases the number of tie molecules between lamellae, reducing crack propagation rate without requiring a lower melt flow rate that would make extrusion impractical.
Environmental stress crack resistance measured on compression-moulded plaques according to ASTM D1693-15e1, Condition B in 10% Igepal CO-630 at 50 °C, is typically reported above 1,000 h F50 for the bimodal resin family; unimodal HDPE grades of equivalent density may fall below 100 h under the same conditions. This difference is relevant for buried pipe in wet, surfactant-containing soils. The resin’s notched pipe response is also influenced by extrusion-induced orientation and cooling stress; a fast-cooled pipe with high frozen-in stress may lose a portion of the crack resistance available in annealed laboratory samples.
Typical extrusion applications for TR571M include pressure water mains, gas distribution pipe, sewage force mains, and industrial slurry lines where long-term hydrostatic strength at 20–60 °C is required. The grade is also extruded into corrugated drainage culverts and protective conduit with carbon black masterbatch added for ultraviolet stabilization. Potable water pipe systems must be certified at the finished-pipe level under EN 12201-1 or ISO 4427-1, including organoleptic and migration tests; the resin alone does not confer system approval. Gas distribution pipe requires rapid crack propagation assessment under ISO 13477:2008 at 0 °C; the critical pressure from the S4 test is compared with the design maximum operating pressure using the safety factor specified in ISO 4437.
| Performance requirement | Standard | Typical test condition |
|---|---|---|
| Hydrostatic pressure resistance | ISO 1167-1:2006 | 12.4 MPa/20 °C/100 h; 10.0 MPa/80 °C/165 h |
| Notched pipe slow crack growth | ISO 13479:2009 | 80 °C/4.0–4.6 MPa |
| Rapid crack propagation S4 | ISO 13477:2008 | 0 °C |
| Finished potable water pipe compliance | EN 12201-1/ISO 4427-1 | Pipe-system certification required |
| Environmental stress crack resistance | ASTM D1693-15e1 | 10% Igepal CO-630/50 °C |
Substitution into an existing line designed for a PE80 or unimodal HDPE pipe grade is not a drop-in change. The bimodal resin’s higher molecular weight can raise head pressure by 5–15% at constant screw speed and temperature profile, requiring reset of the die gap, cooling water flow, and haul-off puller ratio. Wall thickness variation is controlled to ±0.1 mm for standard dimension ratio pipe by adjusting haul-off tension; excessive tension induces frozen-in stress that may reduce slow crack growth resistance. Compared with injection-moulding HDPE grades having MFR above 1.0 g/10 min, TR571M is unsuitable for thin-wall injection moulding because of high viscosity and long cycle times. Compared with film-grade HDPE, this grade has lower melt indices and higher molecular weight, reducing draw-down and increasing hoop stress capacity.
This grade is not crosslinked; it retains melt recyclability but has a continuous-use temperature limit under pressure below 60 °C for many water service conditions. It should not be considered a direct substitute for crosslinked polyethylene or random copolymer polypropylene in hot-water plumbing. Published data for TR571M in PE100-RC configurations is limited; classification as a high stress-crack resistant compound requires validation of the finished pipe and notched pipe test results from the specific extrusion line.
Within the producer’s HDPE portfolio, TR571M is differentiated from blow-moulding grades by its lower MFR and higher environmental stress crack resistance, and from film grades by its lower melt index and higher density. The 0.950 g/cm³ density target is selected to balance pipe ring stiffness and long-term crack resistance; raising density above 0.958 g/cm³ would improve stiffness but degrade slow crack growth resistance. For pressure rating, the resin must be converted to pipe and classified according to ISO 12162:2009 after long-term hydrostatic testing at multiple temperatures. A PE100 classification requires a minimum required strength of 10.0 MPa at 20 °C for 50 years; this is an extrapolated value from test data, not a direct short-term tensile measurement.
Regulatory documentation is obtained from Sinopec Maoming or authorized distributors. The polymer is typically supported under EU REACH regulation 1907/2006, RoHS recast 2011/65/EU, and, for food-contact uses, 21 CFR 177.1520 when the finished article meets the end-use limitations. Potable water approvals are handled at the pipe level under EN 12873-1 or national equivalents. For outdoor service, carbon black masterbatch is recommended at 2.0–2.5 wt% carbon black content to meet ISO 4427-1 requirements for UV resistance; the masterbatch carrier should have a melt flow rate in the range 0.1–0.5 g/10 min to limit viscosity mismatch. Regrind addition from the same grade is commonly limited to 20 wt% for pressure pipe because higher fractions increase viscosity variability and reduce hydrostatic failure time; non-pressure conduit may allow higher fractions if the dimensional and impact properties remain within specification. The use of low-molecular-weight amide slip additives above 0.05 wt% is not recommended because migration to the weld interface can reduce hydrostatic weld strength.