| HS Code | 574695 |
| Density | 0.944 g/cm³ |
| Melt Flow Rate 190c 5kg | 0.25 g/10 min |
| Tensile Yield Strength | ≥23 MPa |
| Elongation At Break | ≥600% |
| Flexural Modulus | ≥1000 MPa |
| Notched Impact Strength | ≥60 kJ/m² |
| Vicat Softening Temperature | ≥120 °C |
| Brittleness Temperature | ≤-70 °C |
| Oxidation Induction Time | ≥20 min |
| Carbon Black Content | 2.0-2.5% |
| Environmental Stress Cracking Resistance | ≥1000 h |
| Minimum Required Strength Mrs | 10.0 MPa |
| Pe Classification | PE100 |
| Color | Black |
| Form | Pellets |
As an accredited Sinopec Maoming HDPE P4406C factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinopec Maoming HDPE P4406C comes in 25 kg polypropylene woven bags, 40 bags per pallet, totaling 1,000 kg. |
| Container Loading (20′ FCL) | Sinopec Maoming HDPE P4406C is packed in 25kg bags, palletized and securely loaded into a 20-foot FCL container for shipment. |
| Shipping | Sinopec Maoming HDPE P4406C is shipped as non-hazardous polyethylene pellets, typically in 25 kg PP woven bags or 1,000 kg jumbo bags. It is palletized or loaded into 20'/40' containers. Store in a dry, ventilated area away from heat and direct sunlight. No special dangerous goods handling required. |
| Storage | Store Sinopec Maoming HDPE P4406C in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, moisture, and ignition sources. Keep original packaging sealed to prevent contamination. Avoid prolonged UV exposure and excessive stacking pressure. Maintain clean handling areas, separate from incompatible chemicals, and rotate stock using first-in, first-out principles. Do not store outdoors. Protect from physical damage. |
| Shelf Life | Shelf life is typically 24 months when stored dry, cool, ventilated, sealed, and away from direct sunlight, moisture, and contaminants. |
Potable water pressure mains based on Sinopec Maoming HDPE P4406C are produced under ISO 4427, EN 12201-1, and GB/T 13663.2, which classify the resin by its minimum required strength under ISO 9080 long-term hydrostatic evaluation. For PE100-class pipe compounds, the MRS is 10 MPa under ISO 12162; the compound is metered at 100 wt% as supplied, without additional carbon black masterbatch, because the black package is already dispersed into the granules. Carbon black content in the finished wall remains 2.0%–2.5% by mass, and dispersion is checked to ISO 18553 with a rating not exceeding 3; recycled in-house trim may be metered up to 15 wt%, provided the same dispersion and density limits are verified after extrusion. Downstream processing on a 65 mm grooved-feed single-screw extruder with L/D 33:1 and a barrier screw achieves a melt temperature between 190°C and 220°C before a spiral mandrel die. Pipe is sized in a vacuum tank, cooled in multi-chamber spray baths, and cut into 6 m or 12 m straight lengths or coiled in 100 m coils for smaller diameters. The terminal products are PE100 potable water mains in DN110–DN630, SDR11 and SDR17 pressure ratings, used for urban distribution and residential service connections. Field observations on production lines show that exceeding 230°C at the adapter shortens oxidative induction time and produces surface scorch defects; therefore barrel temperatures in the feed zone are set to 170°C with progressive zones not exceeding 210°C. Batch-to-batch variation in melt flow at 5 kg load is monitored under ISO 1133-1 to keep die pressure stable and avoid wall thickness oscillation.
Under ISO 4437, EN 1555, and GB 15558.1, gas distribution pipe extrusion from the same PE100-class compound is required to pass fracture-mechanics validation beyond water-pipe standards. The processing formulation uses 100 wt% P4406C; the pre-dispersed carbon black is kept at 2.0%–2.5% by mass to satisfy UV and oxidative stability for outdoor storage, while a 3%–5% HDPE-based yellow masterbatch is introduced through a coextrusion stripe line only, not into the pressure wall. Downstream production uses a grooved-feed extruder with L/D 30:1–36:1, a static mixer in the adapter, and a spiral mandrel die with laser diameter scanning and ultrasonic wall-thickness monitoring. Pipe is cooled in vacuum calibration with closed-loop water temperature at 25°C–35°C, pulled through a caterpillar haul-off, and cut into 12 m lengths or coiled. Terminal products are black PE100 gas mains with coextruded yellow stripes in DN20–DN400, SDR11 and SDR17, butt-fused on site with ISO 21307 fusion parameters. The critical processing boundary is rapid crack propagation control under ISO 13477:2008 and slow crack growth under ISO 13479:2022; excessive melt temperature above 220°C or prolonged residence time degrades the high-molecular-weight tail, shifting the ductile-brittle transition and lowering the full-scale critical pressure. Plant test programs therefore impose a maximum adapter temperature of 220°C, a screw-speed ceiling established by melt-temperature measurement on the selected extruder, and a minimum 24 h conditioning period before notched-pipe testing.
Industrial pressure applications for P4406C are governed by ISO 15494 as the compliance framework for polyolefin industrial pipes, which replaces potable-water hygiene annexes with fluid-resistance and wear documentation. The compounding formulation is 100 wt% P4406C; clean in-house regrind from butt-fusion beads and cut-off ends may be incorporated at up to 10 wt% when the resulting pipe is not intended for potable certification. No mineral fillers, nucleating agents, or external carbon black masterbatches are introduced because the compound’s stabilization and carbon black dispersion are already designed for pressure-pipe extrusion. Downstream processing for thick-wall slurry lines uses a grooved-barrel single-screw extruder with L/D 33:1, a spiral mandrel die, and gravimetric dosing to control wall thickness over SDR 7.4–SDR 17. Multi-chamber vacuum calibration and long cooling sections are required to remove latent heat from wall thicknesses above 40 mm; pulling speed is reduced relative to thin-wall potable pipe to maintain roundness below 2% ovality. The resulting products are butt-fused tailings and dredge discharge lines, process slurry transfer spools, and mine dewatering mains, typically from OD 200 mm to OD 1600 mm, operating at design pressures derived from hydrostatic regression data rather than short-term burst. No published multi-year abrasion data for this exact compound in high-solids slurry service has been identified; end users should validate mass-loss rates against reference PE100 pipe using project-specific slurry loop tests.
| Application | Compliance set | Test method or design basis | Critical process boundary |
|---|---|---|---|
| Potable water distribution | ISO 4427, EN 12201-1, GB/T 13663.2 | ISO 9080 long-term strength, ISO 12162 MRS classification, ISO 1167 hydrostatic strength | Adapter melt temperature ≤220°C; carbon black 2.0–2.5% |
| Gas distribution | ISO 4437, EN 1555, GB 15558.1 | ISO 13477 RCP, ISO 13479 SCG | Melt temperature 190–220°C, post-extrusion conditioning ≥24 h |
| Industrial slurry | ISO 15494 | Hydrostatic regression per material MRS; project slurry loop tests | Wall thickness above 40 mm requires extended cooling; ovality ≤2% |
| Geothermal loops | IGSHPA, CSA C448, EN 12201 | ISO 1167, ISO 9080 design basis | Fusion surface 180–230°C; test pressure 1.5× design for ≥60 min |
| Trenchless slip-lining | ASTM F585, AWWA C906, ISO 11299-1 | ISO 21307 butt fusion | Pull stress ≤50% tensile yield; temporary reduction 5–10% |
| Marine outfall/intake | ISO 4427, EN 12201, BS 6349 | ISO 9080, ISO 21307 | Melt-temperature band to prevent sharkskin; carbon black 2.0–2.5% |
In geothermal ground-loop construction, P4406C is selected primarily for slow crack growth resistance under constant loop temperature and external soil stress, with compliance references drawn from IGSHPA, CSA C448, and the pipe’s pressure rating under EN 12201. The compound is processed at 100 wt%; trimmed U-bend fusion beads and misaligned sockets are discarded rather than reintroduced, since repeated heat history and oxidation reduce ring-tension hydrostatic results even when visual appearance is unchanged. Downstream fabrication steps include butt fusion of straight pipe at 210°C–220°C, socket fusion for branch manifolds, and pressure testing of assembled circuits at 1.5× system design pressure for a duration not shorter than 60 min. U-bends are factory-formed or site-fabricated from DN32, DN40, and DN50 SDR11 pipe. The terminal products are vertical geothermal loop circuits, horizontal slinky-style ground loops, and header manifolds for ground-source heat pump systems. Processing limits are governed by fusion-joint integrity: if the pipe surface temperature falls below 180°C or exceeds 230°C, insufficient melt mixing or excessive melt displacement creates brittle weld zones that are difficult to detect in the field. Long-term published data for this compound in closed-loop geothermal service is limited; the material’s PE100 hydrostatic classification provides the design basis, but soil thermal conductivity and seasonal loop temperature remain design variables outside the resin specification.
Trenchless rehabilitation of buried water and sewer mains uses P4406C in slip-lining applications where the PE100 pressure wall is pulled through an existing host pipe after temporary outside-diameter reduction. The compliance framework includes ASTM F585 for insertion of polyethylene pipe into existing sewers, AWWA C906 for polyethylene pressure pipe in water service, and ISO 11299-1 for trenchless renovation of gas networks where applicable. The formulation remains 100 wt% P4406C; no lubricant or viscosity modifier is added to the compound during pipe production, and field-applied pulling lubricants must be confirmed by the lubricant supplier as non-damaging to PE100 stabilizer packages before use. Downstream processing for liner pipe uses a grooved-feed extruder with a spiral die; the pipe is butt-fused into strings using ISO 21307 low-pressure fusion procedures. During installation, a reducing die compresses the outside diameter by 5%–10% immediately before the pipe enters the host main; after insertion, the PE100 wall relaxes toward the host wall over a period that depends on temperature and prior strain. Terminal products include slip-lined water distribution mains and gravity sewer liners from DN250 to DN1000, refurbishing cracked or leaking host pipes without full excavation. The critical operational boundary is pull force: axial tensile stress during winching must not exceed 50% of the material’s tensile yield strength, and installation records should log both pulling force and tail tension to avoid necking. Tensile yield data specific to P4406C under this installation method is not available in the public domain; the pipe’s ISO 9080-based MRS classification is not a substitute for site-specific pull-force calculation.
For seawater intake and outfall pipelines, the compound is processed into large-diameter PE100 pipe where slow crack growth resistance under submerged external pressure and constant internal flow is the governing material requirement. Compliance for the pipe body remains ISO 4427 and EN 12201; marine structural loading is addressed through BS 6349 for maritime works, and butt fusion follows ISO 21307. The formulation is 100 wt% P4406C; for large-diameter submerged lines, the carbon black package remains at 2.0%–2.5% and no additional anti-fouling or abrasive-resistant fillers are incorporated into the pressure wall. Downstream production involves extrusion of large-diameter pipe from 315 mm to 2000 mm outside diameter with wall thickness governed by the design pressure and sinking calculations. Onshore stringing uses butt fusion; concrete ballast collars are installed at intervals, and the string is floated, towed, and sunk by controlled flooding of the ballast tanks. Terminal products are seawater intake headers, desalination plant outfalls, power plant cooling water lines, and temporary bypass discharge pipelines. The limiting processing factor at these diameters is melt fracture and wall-thickness uniformity; die gap and melt temperature must be held in a narrow band because the high-molecular-weight compound exhibits no flow when underheated and surface sharkskin when over-pushed. Submerged outfall service data for P4406C is limited; the resin’s PE100 hydrostatic classification supports the pressure wall, but marine design loads, current forces, and ballast spacing are governed by civil and marine engineering standards rather than the material datasheet.
Competitive Sinopec Maoming HDPE P4406C prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Maoming HDPE P4406C is a bimodal high-density polyethylene grade manufactured at the Maoming Petrochemical complex. The product is supplied as a black compound or as natural resin for converter-controlled carbon black masterbatch addition. The polymerization design combines a low-molar-mass component that provides shear thinning during extrusion with a high-molar-mass component that contributes melt strength and slow crack growth resistance. This structural balance places the grade in the pressure-pipe segment rather than general-purpose injection or film segments. Lot certificates should be consulted for density, melt flow rate, tensile yield, and oxidation induction time because additive and pellet characteristics vary by campaign.
Current supplier literature positions P4406C within the PE100 hydrostatic design envelope. The PE100 classification is defined through ISO 12162:2009 and requires extrapolated long-term hydrostatic strength of at least 10 MPa at 20 °C for 50 years when tested according to ISO 9080:2022. For water service at 20 °C, the resulting design stress is commonly 8.0 MPa after applying a service coefficient of 1.25; wall-thickness calculations follow ISO 4427-2:2020. The resin classification does not by itself certify finished pipe. System compliance must be demonstrated separately under ISO 4427-1:2019 for water mains, ISO 4437-1:2015 for gas distribution, or equivalent national standards. Batch-to-batch variation in comonomer content and antioxidant package can shift the long-term hydrostatic regression curve, so pipe manufacturers should maintain incoming resin control charts.
The product’s high-molar-mass fraction is produced with a short-chain comonomer, typically 1-butene or 1-hexene. Comonomer type affects slow crack growth resistance because longer short-chain branches on high-molar-mass chains increase tie-molecule density. Hexene-based HDPE pipe grades generally show better slow crack growth resistance than butene-based grades at equivalent density. The specific comonomer system used in P4406C should be confirmed through lot documentation, because the supplier may adjust the comonomer system across production campaigns. Density and branch distribution are reactor-controlled rather than post-reactor blended.
Melt mass-flow rate for the grade is specified in the range 0.20–0.30 g/10 min under a 5 kg load at 190 °C when measured to ISO 1133-1:2022. This low MFR reflects high average molar mass and excludes the resin from thin-wall injection moulding. Single-screw pipe extruders with grooved-feed barrels and 30:1 to 37:1 L/D barrier screws are the practical processing route. Screens of 80–100 mesh remove gels and agglomerates but raise back pressure. At constant screw speed, a 65 mm grooved-feed line may operate at melt pressures of 180–240 bar; the actual value depends on die resistance, screen pack condition, and melt temperature. The broad molecular weight distribution produces strong shear thinning in the die, but the low MFR increases motor torque and residence time relative to film-grade HDPE.
Barrel set points are typically staged from 180 °C in the feed zone to 210 °C in the metering zone, with the die head held at 200–215 °C. Melt temperature measured at the adaptor should remain below 225 °C. Above 230 °C, thermo-oxidative chain scission accelerates and the oxidation induction time measured by ISO 11357-6:2018 may fall below 20 min. A narrow processing window therefore exists at high screw speeds; operators should not compensate for high melt viscosity by raising barrel temperature beyond the antioxidant-limited ceiling. If the melt temperature cannot be held below 225 °C while maintaining output, screw geometry or back-pressure adjustment is required rather than further temperature increase.
Pressure-pipe extrusion requires careful control of melt temperature because of competing requirements: high temperature lowers viscosity and head pressure, but reduces thermo-oxidative stability. In practice, the difference between barrel set point and actual melt temperature can exceed 10 °C at high screw speeds due to viscous dissipation. The operator should therefore use an immersion thermocouple at the adaptor and record pressure at the screen changer. Screen pack blinding raises melt temperature even when barrel zones remain unchanged; a pressure rise of 30 bar across the pack is a practical trigger for screen change. Failure to change screens can cause localized overheating and create black specks from degraded carbon black agglomerates.
Process data from production-scale machines equipped with 65 mm or 75 mm grooved-feed extruders at 33:1 L/D show stable dimensional control when the pipe calibration sleeve is 3–5% smaller than the die bushing diameter. Melt pressure fluctuations of ±10 bar at the breaker plate are typically acceptable; larger fluctuations indicate feed bridging or inconsistent carbon black masterbatch dosing. Surface moisture on pellet stock stored outdoors should be removed at 80 °C for 1–2 h when ambient relative humidity exceeds 60%, because water at the hopper inlet can produce surface pitting in thick-wall pipe. HDPE is not hygroscopic, and internal moisture is rarely the failure source.
Specific capillary rheometry curves for P4406C are not reproduced here because published data for this specific configuration is limited. Processors changing die geometry or screen filtration should request shear-viscosity data measured to ISO 11443 from the supplier and verify the curve on incoming lots. The low MFR and broad molecular weight distribution produce pronounced shear thinning; this is useful in die land regions but complicates low-shear pumping in long adapters.
During startup, the machine should be purged with a lower-viscosity HDPE or dedicated purge compound before introducing P4406C, because the high-molar-mass resin can retain previous-colour residues. During shutdown, the extruder should be cooled under screw rotation at low speed to avoid static degradation in the barrel. Extended residence times above 30 min at melt temperatures above 220 °C increase gel formation and reduce surface quality of the next production run.
Oxidation induction time measured on the compound at 200 °C by ISO 11357-6:2018 is specified at not less than 20 min. This value serves as a processing-stability gate and not as an independent lifetime prediction. Carbon black content in finished pipe for outdoor service is typically 2.0–2.5% by weight according to ISO 6964:2019, with dispersion assessed by ISO 18553:2002. Poor dispersion leads to agglomerate-induced stress concentration and can lower slow crack growth resistance. When the grade is supplied as natural resin and a 40% carbon black masterbatch is used, the converter should add 5.0–6.25% masterbatch by weight to achieve the target final carbon black content. Let-down calculations must be confirmed by ash testing rather than assumed from hopper settings.
| Property | Test method | Indicative value |
|---|---|---|
| Density at 23 °C | ISO 1183-1:2019 | 0.948–0.952 g/cm³ |
| Melt mass-flow rate, 190 °C, 5 kg | ISO 1133-1:2022 | 0.20–0.30 g/10 min |
| Tensile stress at yield, 50 mm/min | ISO 527-2:2012 | ≥22.0 MPa |
| Tensile strain at break | ISO 527-2:2012 | ≥600 % |
| Charpy notched impact at 23 °C, 1eA | ISO 179-1:2010 | ≥18 kJ/m² |
| Oxidation induction time at 200 °C | ISO 11357-6:2018 | ≥20 min |
| Carbon black content, black compound | ISO 6964:2019 | 2.0–2.5 % |
| Notched pipe slow crack growth, 80 °C, 4.5 MPa | ISO 13479:2022 | ≥500 h |
Slow crack growth resistance is the primary performance distinction between P4406C and standard unimodal HDPE film or blow-moulding grades. The bimodal structure places short-chain branches on high-molar-mass chains, increasing tie-molecule density and improving stress-crack resistance. Notched pipe testing under ISO 13479:2022 at 80 °C and 4.5 MPa hoop stress is used as a batch-release or type-test screen; PE100 pipe grades are expected to exceed 500 h before brittle failure. Unimodal injection-moulding HDPE grades with MFR above 1 g/10 min typically show shorter failure times under identical conditions. Published direct comparative data for P4406C against all competing grades is limited; however, the molecular architecture difference is measurable through molar mass distribution and notched pipe performance.
Compared with high-flow HDPE injection grades in the 50–80 g/10 min MFR range, P4406C has substantially higher melt viscosity and longer residence-time sensitivity. Compared with medium-density film grades with density below 0.940 g/cm³, the resin is denser and stiffer but less suited to thin-gauge blown film because low MFR reduces bubble stability at drawdown ratios above 3:1. The material should not be diluted with high-flow HDPE to improve processing; blending reduces slow crack growth resistance and can invalidate long-term hydrostatic classification.
Reformulation from a standard unimodal HDPE with melt flow rate of 1–4 g/10 min to P4406C requires adjustment of barrel temperature, screw speed, and melt filtration. The low MFR increases specific energy input and residence time; operators should monitor adaptor melt temperature rather than barrel set points. On a 65 mm grooved-feed extruder, head pressure may rise by 20–40 bar under identical screw speed, and output may become torque-limited if the drive system is not sized for high-viscosity pipe resin. The benefit is higher melt strength, which reduces sag in large-diameter thick-wall pipe during vacuum sizing. The resin is not a direct substitute for injection-moulding HDPE or thin-wall blow-moulding HDPE because the low MFR limits flow length and accelerates freeze-off in thin sections.
Fabrication by butt fusion uses heater plate temperature of 200–220 °C and joining sequences defined in ISO 21307:2017. Electrofusion joining requires scraped, clean pipe surfaces and temperature-compensated controls. Because P4406C is a high-molar-mass material, joints must cool to ambient temperature before hydrostatic pressure testing; premature pressurization can create brittle interfacial failure. Welding parameters are pipe-system variables, not resin specifications, and must be validated on finished pipe assemblies. Additive packages containing unapproved amines or incompatible phenolic antioxidants should be avoided without compatibility testing because antioxidant antagonism can reduce oxidation induction time below the 20 min specification.
Base polyolefins are generally outside the scope of RoHS restricted substances, but pipe compound compliance depends on carbon black dispersion and antioxidant chemistry. A REACH Article 33 declaration should be requested from the supplier when the finished pipe is placed on the European market. For drinking-water contact, the relevant approvals are system-specific; resin certification alone does not replace pipe testing under national health regulations.
Incoming resin testing should include melt flow rate, density, tensile yield, and oxidation induction time from each silo or truck delivery. A change in melt flow rate of ±0.03 g/10 min is usually within specification but may require screw-speed adjustment. Density shifts of ±0.002 g/cm³ can affect pipe stiffness and long-term creep; these values should be trended on statistical process control charts. Carbon black content on black compound should be tested per ISO 6964:2019 on a dry sample because moisture affects ashing results.
Storage in sealed silos or original packaging away from direct sunlight preserves lot uniformity. Lot-to-lot variation in melt flow rate and density is expected within the specification envelope; extrusion parameters should be adjusted based on certificate values rather than fixed temperatures. The material is not intended for direct food-contact use unless the finished pipe system is certified under applicable national or regional drinking-water standards. NSF/ANSI 61 or equivalent approvals apply to the finished pipe product, not to the resin alone.