| HS Code | 155050 |
| Grade | Sinopec Hainan HDPE F5703-S(HN7000) |
| Polymer Type | High Density Polyethylene (HDPE) |
| Density | 0.957 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 7.0 g/10 min |
| Tensile Yield Strength | ≥24 MPa |
| Tensile Break Strength | ≥20 MPa |
| Elongation At Break | ≥500% |
| Flexural Modulus | ≥1000 MPa |
| Notched Izod Impact Strength | ≥30 kJ/m² |
| Vicat Softening Temperature | ≥124 °C |
| Hardness | ≥60 Shore D |
| Melting Point | 130-135 °C |
| Crystallinity | 70-80% |
| Environmental Stress Cracking Resistance | ≥1000 h |
| Water Absorption | ≤0.01% |
| Bulk Density | ≥0.55 g/cm³ |
| Volume Resistivity | ≥10^16 Ω·cm |
| Dielectric Constant | 2.3 |
| Ash Content | ≤0.05% |
| Thermal Deformation Temperature | ≥80 °C |
| Brittleness Temperature | ≤-70 °C |
| Form | Pellets |
| Color | Natural |
As an accredited Sinopec Hainan HDPE F5703-S(HN7000) factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinopec Hainan HDPE F5703-S(HN7000) typically comes in 25 kg PP woven bags, 1,000 kg per pallet. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): Sinopec Hainan HDPE F5703-S(HN7000) in 25kg bags, 18MT per container, loose in dry container. |
| Shipping | Sinopec Hainan HDPE F5703-S (HN7000) is shipped as non-hazardous polyethylene pellets in 25 kg woven bags, jumbo bags, or bulk. Transport in clean, dry trucks, railcars, or containers. Keep packages sealed, away from moisture, direct sunlight, heat, and contamination. Handle with standard forklifts; no special dangerous-goods labeling required. |
| Storage | Store Sinopec Hainan HDPE F5703-S(HN7000) in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, sparks, flames, and strong oxidizers. Keep original bags or containers closed, palletized, and off the floor to prevent moisture and contamination. Avoid prolonged UV exposure and excessive stacking. Maintain clean handling areas; follow local regulations and SDS recommendations. Use first-in, first-out stock rotation. |
| Shelf Life | Typically 24 months when stored unopened in a cool, dry, ventilated area, away from direct sunlight, moisture, and contamination. |
High-density polyethylene grade Sinopec Hainan HDPE F5703-S (HN7000), with a nominal melt flow rate of 0.35 g/10 min under ISO 1133-1:2022 and density of 0.950 g/cm³ under ISO 1183-1:2019, is processed as the primary layer in high-strength retail carrier-sack film. Industry compliance for this segment is anchored to ASTM D882-18 for tensile properties and ASTM D1709-22 Method A for dart impact, while European packaging environmental requirements specify compliance with REACH and 94/62/EC. In a typical monolayer formulation, F5703-S constitutes 85 wt% of the compound, with 12 wt% butene-LLDPE added to improve seal initiation and 3 wt% white or print-receptive masterbatch; the LLDPE fraction is not increased beyond 15 wt% because machine-direction film modulus drops below 500 MPa and bag handle-loop tensile strength deteriorates. Downstream manufacturing employs high-stalk blown film extrusion with a die diameter of 300–400 mm, die gap 1.4 mm, blow-up ratio 4:1, and melt temperature 185–205 °C; frost-line height is maintained at 700–900 mm to preserve transverse direction toughness. Production-scale lines equipped with internal bubble cooling and a 25:1 L/D single-screw extruder show that screw speeds above 90 rpm can generate melt pressure fluctuation exceeding ±10 bar unless a melt pump is installed. Terminals converted on side-weld bag machines at sealing temperatures of 140–155 °C include T-shirt carrier sacks, lightweight produce bags, and small retail boutique bags with printed surface areas up to 60%.
In heavy-duty industrial refuse-sack and liner production, the high molecular weight distribution of F5703-S supports gauge reduction without losing tear resistance, but only within a defined process envelope. The governing compliance framework for finished industrial sacks includes tensile testing under ISO 527-3:2018, dart impact under ASTM D1709-22 Method B, and tear propagation under ASTM D1922-15. A validated production formulation for 60–100 µm industrial liner film comprises 75 wt% virgin F5703-S, 23 wt% clean post-industrial HDPE regrind, and 2 wt% carbon black masterbatch with 40% pigment loading; raising the regrind fraction above 25 wt% lowers notched Elmendorf tear in the transverse direction below 18 g and increases dart-impact failure by approximately 20% on a 350 mm die line. The downstream process uses a grooved-feed single-screw extruder with L/D 30:1, barrel temperature profile 160/180/195/205/210 °C, die gap 1.8 mm, blow-up ratio 2.8:1, and dual-lip air ring cooling. At film thickness below 50 µm, melt pressure of 220–260 bar is required to maintain throughput; above 280 bar, screw wear accelerates and surface melt fracture begins as shark-skin banding on the outer bubble surface. Terminal products include construction debris sacks, industrial waste liners, heavy-duty refuse sacks, and high-gauge liners for wet waste collection.
Food-contact monolayer cereal liner and snack packaging use demands strict organoleptic neutrality. F5703-S in virgin form is evaluated for food-contact suitability under FDA 21 CFR 177.1520(c)(1.1), European EU Regulation 10/2011 with overall migration below 10 mg/dm², and China GB 4806.7-2016. The formulation for this segment is limited to 100 wt% virgin resin with 0.8–1.2 wt% inert silica antiblock masterbatch; no post-consumer recyclate is added because migration modelling cannot validate the source stream under the required worst-case food simulants. Processing is carried out on a three-layer blown film line with die gap 1.2 mm, blow-up ratio 2.5:1, melt temperature 190–200 °C, and internal bubble cooling; downstream conversion includes surface corona treatment to 38–42 mN/m and flexographic printing with low-odour water-based inks. Terminal products include boxed cereal liners, frozen-food inner liners, bakery overwrap, and paper-like snack pouches.
| Parameter | Test method | Typical limiting value |
|---|---|---|
| Overall migration | EN 1186-1:2002 | < 10 mg/dm² |
| Heavy metal release | GB 4806.7-2016 | compliant |
| Density | ISO 1183-1:2019 | 0.950 g/cm³ |
When heavy-duty sack film is produced in a three-layer A/B/A structure, post-consumer recyclate is isolated in the core layer while virgin F5703-S forms the outer skins. The relevant compliance framework includes ISO 14021:2016 for recycled content claims, ISO 527-3:2018 for mechanical values, and ASTM D1922-15 for tear propagation. The structure uses skin A at 18 wt% virgin F5703-S, core B at 64 wt% total consisting of 48 wt% F5703-S and 52 wt% post-consumer HDPE flake, and skin C at 18 wt% virgin F5703-S; the overall recycled fraction is therefore 33 wt%. Processing on an A/B/A blown-film line uses two 65 mm skin extruders and one 90 mm grooved-feed core extruder, each with L/D 30:1; the core melt passes through a 100 mesh continuous screen changer and melt pump before entering the multilayer die at 210 °C. Die gap is 1.6 mm, blow-up ratio 2.6:1, and output is adjusted to maintain a core-to-skin viscosity ratio below 1.8:1. Production audits show that when core recycled fraction exceeds 60 wt%, screen-pack pressure rises more than 1.5 bar/hour due to gel and contaminant accumulation, and die-lip deposit formation shortens run cycles. Terminal products include chemical powder sacks, fertiliser valve sacks, resin packaging liners, and moisture-barrier replacement structures requiring water vapour transmission below 1.5 g/m²/day at 38 °C/90% RH.
Blown-film substitution for cast base webs in textile and lightweight moisture-barrier packaging is justified only when surface friction resistance and print adhesion are primary requirements. Compliance is governed by ASTM D2578-23 for wetting tension, ISO 527-3:2018 for mechanical values, and ISO 1133-1:2022 for incoming melt-flow verification. A laminating base formulation contains 70 wt% F5703-S and 28 wt% LDPE grade with 0.35 g/10 min MFR, plus 2 wt% synthetic silica antiblock masterbatch; the LDPE fraction shifts the seal initiation temperature downward to 112–118 °C. The process uses high-stalk blown film with a 250 mm die, 1.2 mm die gap, blow-up ratio 3.2:1, frost-line height 600 mm, and downstream corona treatment at 42 mN/m. Because lamination requires a stable surface energy within 4 mN/m across the roll, inline corona output is adjusted continuously and the film is wound at 450–550 N web tension. Published comparative data for this specific blown-web substitution using HN7000 is limited; converter trial records indicate that the wetting-tension window above is process-specific rather than a single universal setting. Terminal products include BOPP-laminated gift wrap substrate, textile overwrap, and metalised barrier film base for non-food industrial packaging.
Monolayer household bin-liner extrusion constitutes the highest-volume production segment for F5703-S. Standard compliance for dimensional stability and mechanical performance in household refuse sacks is measured under ASTM D882-18 and ASTM D1709-22 Method A, and the European product safety regime for non-food contact plastics requires compliance with REACH Annex XVII. The compound is formulated at 100 wt% F5703-S with 1.8–2.2 wt% low-dust carbon black masterbatch and 0.10–0.15 wt% fluoroelastomer processing aid; masterbatch addition above 2.5 wt% reduces tensile yield strength below 21 MPa and creates film splitting at side-seal edges. Production lines utilise a 350 mm spiral mandrel die, die gap 1.5 mm, blow-up ratio 3:1, melt temperature 180–205 °C, and nip speed set to produce 18–25 µm film. Field audits on three-shift operations show that melt pressure fluctuation should be maintained within ±8 bar; excursions above ±14 bar cause visible gauge bands and increase side-weld leaker rates to 4–6 per 1,000 sacks. Terminal products include kitchen bin liners, janitorial refuse sacks, and light industrial waste bags.
Competitive Sinopec Hainan HDPE F5703-S(HN7000) prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Hainan HDPE F5703-S(HN7000) is a bimodal high-density polyethylene film resin produced on the Hostalen ACP slurry polymerization unit at the Hainan Refining & Chemical complex. The F5703-S designation identifies the compounded film grade containing internal slip and antiblock additives; HN7000 identifies the bimodal reactor base. The resin is specified for high-strength blown film and downgauged packaging where film thickness is reduced below 40 µm and where conventional unimodal high-density polyethylene grades fail to maintain dart impact and tear propagation resistance. Producer documentation lists a nominal density of 0.956 g/cm³ under ISO 1183-1:2019, a high-load melt flow rate of 8.0 g/10 min at 190 °C/21.6 kg under ISO 1133-1:2022, and a 2.16 kg melt flow rate below 0.10 g/10 min. These values place the material in the high-molecular-weight HDPE film category and define its primary differentiation from low-molecular-weight extrusion coating or injection molding grades.
Table 1 consolidates the nominal property set used for incoming resin verification. The values are not a specification; lot-specific certificates of analysis must be obtained for release decisions.
| Property | Test method | Nominal value |
|---|---|---|
| Density | ISO 1183-1:2019 | 0.956 g/cm³ |
| High-load melt flow rate | ISO 1133-1:2022 | 8.0 g/10 min |
| Melt flow rate at 190 °C/2.16 kg | ISO 1133-1:2022 | 0.05 g/10 min |
| Tensile yield stress | ISO 527-2/1B | 27 MPa |
| Elongation at break | ISO 527-2/1B | >600% |
| Dart drop impact, 25 µm film | ASTM D1709A | 300 g–350 g |
| ESCR, 100% Igepal CO-630, F50 | ASTM D1693B | >100 h |
The Hostalen ACP process synthesizes a bimodal molecular weight distribution by combining two polymerization environments. The high-molecular-weight fraction introduces the long chains responsible for tie-molecule formation between lamellae. The low-molecular-weight fraction acts as an internal processing aid by reducing shear viscosity at film extrusion rates. This architecture produces a measurable difference in mechanical behavior: the tensile yield stress is 27 MPa under ISO 527-2/1B, elongation at break exceeds 600%, and the 25 µm monolayer dart drop impact is 300 g to 350 g under ASTM D1709A. Environmental stress crack resistance tested at 50 °C with 100% Igepal CO-630 exceeds 100 h under ASTM D1693B. A unimodal HDPE film grade of equivalent density typically falls below this dart impact threshold because the chain-length distribution lacks enough long-chain tie molecules.
Blown film conversion of F5703-S(HN7000) is normally run on grooved-feed single-screw extruders with L/D ratios of 30:1 to 38:1 and barrier screws with a Maddock mixing section. Barrel temperature profiles from 180 °C to 210 °C and die-head temperatures from 190 °C to 210 °C maintain melt temperatures between 195 °C and 210 °C. The melt pressure upstream of the screen pack should be kept below 320 bar. Sustained pressure above this value is observed on production lines when screen blinding occurs or when the barrel temperature is set below 180 °C; the result is reduced output and gel formation from thermally degraded high-molecular-weight chains at the screw tip.
Bubble stability is optimized at die gaps of 1.2 mm to 1.8 mm and blow-up ratios from 3:1 to 5:1. Frost line height for 30 µm film is typically set between 600 mm and 800 mm to balance MD and TD tear. At a die gap of 1.4 mm and a blow-up ratio of 4:1, the 1% secant modulus in the machine direction exceeds 900 MPa under ISO 527-3. Excessive drawdown reduces transverse tear because orientation locks the high-molecular-weight chains in the machine direction before adequate cross-direction orientation can develop.
The operating window in Table 2 is derived from pilot-line data on a 75 mm grooved-feed extruder with 38:1 L/D and a 250 mm die. Transfer to production equipment should occur only after confirmation of die geometry and cooling air uniformity.
| Parameter | Range | Limiting observation |
|---|---|---|
| Barrel temperature zone 1 | 180 °C–190 °C | Below 180 °C: high screw torque |
| Die-head temperature | 190 °C–210 °C | Above 220 °C: oxidation risk |
| Melt temperature | 195 °C–210 °C | Melt fracture below 195 °C |
| Die gap | 1.2 mm–1.8 mm | Below 1.0 mm: shark-skin melt fracture |
| Blow-up ratio | 3:1–5:1 | Above 5:1: bubble instability |
| Melt pressure before screen pack | 220 bar–320 bar | Above 320 bar: screen blinding |
The viscosity profile of F5703-S(HN7000) is highly shear-sensitive. The 21.6 kg high-load melt flow rate of 8.0 g/10 min does not indicate a low melt viscosity at film extrusion shear rates; it reflects the response of the bimodal distribution under high-shear flow. At the die lip, the resin retains sufficient melt strength for bubble stability at blow-up ratios up to 5:1. However, the same long-chain fraction that provides melt strength raises die pressure. On a 75 mm grooved-feed extruder with 38:1 L/D, die pressures between 220 bar and 280 bar are typical at outputs of 120 kg/h to 180 kg/h for a 250 mm die. The operating window narrows when the die gap is reduced below 1.0 mm: melt fracture becomes visible as shark-skin on the bubble surface and the maximum stable output drops. Increasing the melt temperature above 220 °C resolves melt fracture but accelerates oxidative chain scission; the stabilizer package in F5703-S is not designed for prolonged residence times above this threshold.
The melt flow ratio between the 21.6 kg value and the 2.16 kg value is approximately 160; this ratio is an indirect indicator of bimodality. A reduction below 130 on a processed sample may indicate thermal degradation or contamination with a lower-molecular-weight HDPE. This ratio can be used as an incoming quality check after pelletizing but not as a substitute for film appearance testing.
The additive package in F5703-S includes slip and antiblock agents that affect film-to-film friction and reel handling after conversion. The package is internal, but converters adding external lubricants should limit the total slip-agent concentration because migration of excess erucamide or oleamide can create plate-out on the collapsing frame after 8 h to 12 h of continuous operation. This plate-out is not a resin failure but a process interaction that is controllable by maintaining die-head cleanliness and avoiding incompatible external additives.
In high-density polyethylene film extrusion, gel formation may originate from the high-molecular-weight fraction if the screw has an aggressive barrier clearance below 0.5 mm or if residence time exceeds 10 min at melt temperatures above 210 °C. Production experience on 65 mm and 75 mm extruders shows that lowering the screw speed without lowering the heater setpoints increases melt temperature by shear heating; the result can be fish-eye gels that are not present in the pellets. The recommended corrective action is to reduce barrel temperatures by 5 °C to 10 °C in zones 2 and 3 rather than increasing screw cooling, which can starve the metering section.
In coextruded structures, F5703-S(HN7000) serves as the stiff core layer in 3-layer A/B/A lineups where the skin layers are LLDPE or LDPE. The HDPE core contributes modulus and moisture barrier, while the LLDPE skins contribute heat-seal initiation below 105 °C. Seal strength and hot tack are controlled by the skin layer, not by the HDPE core. Film structures with a 20 µm core of F5703-S and 5 µm skin layers on each side have been evaluated for dry-food form-fill-seal packaging at sealing pressures of 0.5 N/mm² and dwell times of 0.5 s to 1.0 s. Published data for this specific configuration is limited; converter sealing trials are required because the mineral-filled antiblock package can influence seal initiation temperature when the core is present near the interface.
For cereal liners and light-duty shopping bags, downgauging to 12 µm or 15 µm is possible only when the film line has dual-lip air ring cooling and automatic gauge control. Monolayer lines without internal bubble cooling often exhibit gauge scatter at these thicknesses, and the dart impact advantage of the bimodal resin is lost to thickness variation. The 1% secant modulus of 900 MPa to 1100 MPa under ISO 527-3 provides stacking strength, but the film must be cooled rapidly to maintain the frost line at the calibrated height; otherwise the bubble sags and transverse gauge profiles widen.
Sinopec Hainan’s 5000S grade is a blow-molding HDPE with lower high-load melt flow and a different molecular architecture. It is not interchangeable with F5703-S in film applications because its dart impact on 25 µm film is lower and its bubble stability at high blow-up ratios is insufficient. Compared with a conventional unimodal HDPE film grade of similar density, F5703-S(HN7000) provides higher dart impact and better environmental stress crack resistance at equivalent film thickness. The difference is process-intensive: the bimodal low-molecular-weight fraction allows higher screw speeds without excessive torque, while the high-molecular-weight fraction retains mechanical properties during downgauging. This bimodal advantage is measurable as an increase in dart impact from approximately 150 g to 250 g for a unimodal grade to 300 g to 350 g for F5703-S under the same ASTM D1709A test on 25 µm film.
Compared with metallocene linear low-density polyethylene, F5703-S(HN7000) has higher 1% secant modulus, lower elongation at break, and lower low-temperature puncture resistance. The stiffness of F5703-S is exploited in light-duty shopping bags and cereal liners where low creep at elevated stack loads is required. The resin is not suitable for high-speed stretch film or frozen-food bags requiring the low-temperature toughness of mLLDPE; the lower low-temperature dart impact is a property boundary, not a processing defect.
The parenthetical HN7000 designation is used in product certificates to identify the base reactor grade, while the F5703-S suffix identifies the compounded film formulation. Converters that require a custom slip/antiblock level should request the base grade and add a masterbatch; the pre-compounded F5703-S version reduces dosing variability but limits flexibility for high-clarity applications because the antiblock component raises haze. Haze values for 50 µm film are typically above 20% under ISO 14782, making the grade unsuitable for clear display film.
The pellets are supplied in 25 kg bags or bulk containers. Storage should be in dry, ventilated warehouses below 30 °C and protected from ultraviolet exposure. Polyethylene is hydrophobic, but the slip/antiblock package can adsorb surface moisture at relative humidity above 60%; if pellets are stored in open bags under these conditions, surface moisture can produce bubble instability and pinhole defects during film conversion. In such cases, pre-drying at 70 °C to 80 °C for 4 h is sufficient. The resin should not be exposed to flame or temperatures above 300 °C; thermal decomposition begins above 350 °C.
Film property testing should condition specimens at 23 °C and 50% relative humidity for at least 40 h under ISO 291. The dart drop test under ASTM D1709A is sensitive to film gauge and test temperature; a thickness deviation of ±2 µm can shift the measured impact by 10% to 15%. Incoming film certification should include online gauge profiling rather than relying solely on roll-average thickness. Tear tests under ISO 6383-2 should be reported with both MD and TD values because unequal orientation produces anisotropy that can be mistaken for resin variability.
Food-contact compliance for the base polymer can be referenced to FDA 21 CFR 177.1520 for olefin polymers. European Union food-contact evaluation requires the converter to verify migration under Regulation (EU) No 10/2011 and its amendments for the actual film structure and food simulant. F5703-S(HN7000) is not supplied as a medical-grade polymer; use in drug primary packaging or implantables would require additional supplier validation and regulatory testing beyond the standard film resin certificate.