| HS Code | 741828 |
| Density | 0.950 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 0.75 g/10 min |
| Melting Point | 130-135 °C |
| Vicat Softening Point | 120-125 °C |
| Tensile Strength At Yield | ≥25 MPa |
| Tensile Strength At Break | ≥30 MPa |
| Elongation At Break | ≥500% |
| Flexural Modulus | ≈1000 MPa |
| Environmental Stress Cracking Resistance | >1000 h |
| Impact Brittleness Temperature | <-70 °C |
| Water Absorption | <0.01% |
| Film Haze | ≤12% |
| Film Gloss | ≥50% |
| Dart Impact Strength | ≥80 g |
| Hardness Shore D | ≈65 |
| Volume Resistivity | >10^16 Ω·cm |
| Dielectric Constant 1 Mhz | ≈2.3 |
| Dissipation Factor 1 Mhz | <0.0005 |
| Molecular Weight Distribution | Broad |
| Crystallinity | 70-80% |
As an accredited Sinopec Fujian HDPE FI0750 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinopec Fujian HDPE FI0750 comes in 25 kg woven bags with inner liners, typically palletized or stacked for shipment. |
| Container Loading (20′ FCL) | Container loading (20′ FCL): Sinopec Fujian HDPE FI0750 in 25 kg bags, palletized, shrink-wrapped, and securely stowed for sea freight. |
| Shipping | Sinopec Fujian HDPE FI0750 is a non-hazardous polyethylene resin, typically shipped in 25 kg PP woven bags or 1,000 kg jumbo bags, palletized for transport. It moves in dry, ventilated containers or trucks, protected from moisture, sunlight, and contamination. No dangerous-goods classification applies; store cool and dry. |
| Storage | Store Sinopec Fujian HDPE FI0750 in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and strong oxidizers. Keep original packaging sealed, palletized, and protected from moisture, dust, and contamination. Avoid static discharge and ignition sources. Do not store outdoors or near incompatible substances. Stack securely and follow manufacturer SDS, local regulations, and first-in, first-out rotation. |
| Shelf Life | Shelf life is generally 12 months when stored in original, unopened packaging under dry, cool, ventilated conditions away from sunlight. |
In thin-wall dairy pot and deli tray injection moulding, high-flow HDPE FI0750 is used as a single-resin injection stream with a closed-loop regrind fraction of 10–15 wt%; the selection is driven by a melt mass-flow rate of 7.5 g/10 min at 190°C under 2.16 kg according to ISO 1133-1:2022. Compliance for direct food contact follows Regulation (EU) No 10/2011 with an overall migration limit of 10 mg/dm² into aqueous, acidic and fatty food simulants, and FDA 21 CFR 177.1520(c) for US-bound articles under Conditions of Use A through H; the Chinese market reference is GB 4806.6-2016. Formulation addition on the production floor is 1.5–3.0 wt% TiO₂ white masterbatch and 0.05–0.15 wt% fluoropolymer processing aid, with tinted pots holding total organic or carbon black pigment below 0.5 wt% to avoid exceeding the migration threshold. The downstream manufacturing process is high-cavitation injection moulding with hot-runner valve gating, melt temperature 210–240°C, mould coolant at 8–18°C, filling speed 80–140 mm/s, hold pressure 45–70 MPa, and clamping force 150–450 t depending on cavitation. Terminal products are dairy pots, single-serve dessert cups, and thin-wall deli/insert trays. The upper temperature limit is critical: melt-temperature excursions above 250°C and residence time longer than 3 min can cause oxidative chain scission, volatile aldehyde generation and gate blush in high-shear zones.
| Application | Standard/code | Test criterion | Acceptance indicator |
|---|---|---|---|
| Thin-wall dairy containers | EU No 10/2011 | Overall migration | 10 mg/dm² |
| Thin-wall dairy containers | FDA 21 CFR 177.1520(c) | Use condition | Conditions A–H |
| Caps and closures | ASTM D2063/D2063M-12(2020) | Torque retention | Application-specific |
| Industrial pails | UN 1H2/Y | Drop/stack/leak | SG 1.5 |
| Industrial pails | ISO 2234:2000 | Stacking static load | No closure failure |
| Logistics crates | REACH | SVHC per article | <0.1 wt% |
| Returnable pallets | ISO 8611-1:2021 | Compression/bending | Client-specific |
Closure production with FI0750 is organized around multi-cavity hot-runner tools with sequential valve gates, because the nominal melt mass-flow rate of 7.5 g/10 min at 190°C/2.16 kg according to ISO 1133-1:2022 permits short fill without excessive injection pressure. Compliance includes FDA 21 CFR 177.1520, EU No 10/2011 for food simulant migration, and ASTM D2063/D2063M-12(2020) for torque retention on continuous-thread closures. Additive ratios on the cap line are 1.5–2.5 wt% colour masterbatch, 0.05–0.10 wt% mould release, and 0.06–0.12 wt% primary antioxidant masterbatch; erucamide slip is restricted to below 0.05 wt% when the cap must pass low-torque opening, oxygen-barrier liner adhesion, or organoleptic testing. The process operates at melt temperature 220–250°C, hot-runner tip temperature 240–260°C, mould water temperature 10–20°C, injection pressure 80–120 MPa, hold pressure 35–60 MPa, and cooling time 4–9 s in 48- to 96-cavity tools. Terminal product types are PCO 1881 beverage bottle caps, HDPE condiment closures, and tamper-evident snap-hinge caps. Gate vestige height is controlled at ≤ 0.15 mm by valve-pin geometry and pack-pressure profile to prevent cap top-face interference in automatic capping heads.
A 20-L open-top pail moulded from FI0750 operates under stack-loading conditions where wall thickness and handle-boss integrity determine warehouse compression survival. For dangerous-goods shipments, the pail must meet UN 1H2/Y performance requirements for liquids up to specific gravity 1.5; for non-dangerous paint and lubricant pails, compressive strength is evaluated to ISO 2234:2000 or ASTM D4577-19 under sustained top load. The formulation includes 15–30 wt% closed-loop post-industrial regrind, 0.2–0.5 wt% high-molecular-weight HALS stabilizer, 0.08–0.15 wt% processing antioxidant, and 2.0–3.0 wt% carbon black masterbatch for ultraviolet resistance; regrind contamination with polypropylene above 2 wt% is rejected because it narrows the weld-line strength at the handle boss. The downstream manufacturing route is injection moulding on machines of 600–1200 t clamp force, with melt temperature 200–230°C, mould temperature 8–16°C, injection pressure 75–110 MPa, packing pressure 45–65 MPa for 5–12 s, and core cooling 18–28 s before ejection. Terminal products are 5-L, 10-L, and 20-L open-top pails and lidded containers used for paints, coatings, greases, detergents and low-risk chemical filling.
Logistics crate and tote moulding for returnable transit packaging places impact toughness and top-load retention ahead of cosmetic surface finish; the required property set is secured by blending FI0750 with post-industrial recycled HDPE at 30–50 wt% and adding 3–6 wt% polyolefin elastomer impact modifier plus 1.5–2.5 wt% colour masterbatch. The regulatory basis for non-food industrial crates is Regulation (EC) No 1907/2006 (REACH) and, when the crate is sold into electrical/electronic logistics chains, Directive 2011/65/EU (RoHS) for restricted substances. Processing on multi-gate injection moulding machines with clamp force 500–900 t uses melt temperature 210–250°C, hot-runner manifold temperature 220–245°C, injection speed profile 60–140 mm/s, packing pressure stepped from 70 MPa to 30 MPa over 8–12 s, and cooling time 20–35 s. Terminal product types include dairy crates, bread trays, beverage crates, and collapsible distribution totes. Published data for the exact FI0750/recycled-HDPE mechanical blend under wet-cold crating cycles is limited; plant-level drop impact at −10°C is required before tool transfer.
| Application | Formulation addition ratio | Melt temperature | Mould temperature | Terminal product type |
|---|---|---|---|---|
| Thin-wall dairy containers | 1.5–3.0 wt% TiO₂ masterbatch; 0.05–0.15 wt% processing aid | 210–240°C | 8–18°C | Dairy pots, deli trays |
| Caps and closures | 1.5–2.5 wt% colour masterbatch; 0.06–0.12 wt% antioxidant | 220–250°C | 10–20°C | PCO 1881 caps, condiment closures |
| Industrial pails | 15–30 wt% regrind; 2.0–3.0 wt% carbon black masterbatch | 200–230°C | 8–16°C | 5-L, 10-L, 20-L pails |
| Logistics crates | 30–50 wt% recycled HDPE; 3–6 wt% POE | 210–250°C | 10–20°C | Dairy crates, beverage crates, totes |
| Storage bins | 10–20 wt% regrind; 1.0–2.0 wt% masterbatch | 210–240°C | 10–20°C | Household storage boxes, organizers |
| Returnable transport packaging | 20–40 wt% recycled HDPE; 4–8 wt% impact modifier | 220–250°C | 10–18°C | Pallet feet, deck panels, trays |
Because storage bin sidewalls are long-flow, thin-gauge surfaces, gate filling imbalance dominates dimensional stability and pallet-fit tolerances. In this non-food consumer-goods sector, compliance is governed by REACH and, for articles exported to California, Proposition 65 chemical disclosure requirements. The formulation added at the moulding machine is 1.0–2.0 wt% masterbatch, 0.05–0.10 wt% fluoropolymer processing aid, and 10–20 wt% internally generated regrind; external mould release is excluded because it deposits on vent slots and increases warp at gate convergence zones. The production route uses high-speed injection moulding with sequential valve-gated cold-runner sprues, melt temperature 210–240°C, mould temperature 10–20°C, fill time 1.5–3.5 s, and hold pressure 40–60 MPa. Terminal products are household storage boxes, drawer organizers, and under-bed storage units with wall thickness from 1.2 mm to 2.4 mm.
Returnable transport packaging for regulated supply chains requires environmental stress-cracking resistance (ESCR) while maintaining flow sufficient for long gas channels. The relevant palette standard for pallet components is ISO 8611-1:2021; for food-transit crates, EC 1935/2004 applies to the article, not solely to the resin, and FDA 21 CFR 177.1520 applies only when the packaging directly contacts food. The formulation combines 20–40 wt% recycled HDPE, 4–8 wt% metallocene polyolefin impact modifier, 0.1–0.3 wt% hindered phenolic antioxidant, and 1.5–2.5 wt% carbon black masterbatch; the recycled fraction is selected from lower-melt-index HDPE to partially offset the ESCR penalty of high-MFR FI0750. Published Bell-test data for this exact blend configuration are limited; plant-level ESCR screening under ASTM D1693-15 is therefore performed at 50°C in 100% Igepal CO-630 before tool transfer. The gas-assisted injection moulding process uses nitrogen gas pressure 10–25 MPa, melt temperature 220–250°C, mould temperature 10–18°C, injection fill time 3–8 s, and gas delay time 1.0–2.0 s. Terminal products are pallet feet, top deck panels, corner blocks and returnable transport trays. Gas-channel walls below 4 mm should be avoided when pallets are stored outdoors below 0°C.
Competitive Sinopec Fujian HDPE FI0750 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinopec Fujian HDPE FI0750 is an injection-moulding high-density polyethylene resin supplied by Sinopec Fujian Refining & Chemical Co., Ltd. The grade is controlled to a nominal melt mass-flow rate of 7.5 g/10 min measured at 190 °C under 2.16 kg load in accordance with ISO 1133-1:2022, and a nominal density of 0.956 g/cm³ determined by ISO 1183-1:2019. The combination of moderate melt flow and high crystallinity places the material in the rigid injection-moulding segment for short-cycle production of containers, caps, crates, pallets and technical parts requiring stiffness and dimensional stability. Because the polymer is an ethylene homopolymer with a low degree of short-chain branching, the solid-state structure is dominated by tightly packed orthorhombic crystallites; this accounts for the density approaching the crystalline limit and for the relatively high flexural modulus observed in moulded plaques.
The product is typically characterised by a tensile yield stress in the range 24–28 MPa when tested at 50 mm/min according to ISO 527-2:2012, a flexural modulus of approximately 1,100 MPa under ISO 178:2019, and a notched Izod impact strength at 23 °C of 4–6 kJ/m² under ISO 180/A:2023. Vicat softening temperature is commonly reported near 123 °C using ISO 306/A120. Tensile elongation at break is generally above 200 %. These values should be read as technical-bulletin ranges rather than batch-certificate limits; converter validation is required for critical dimensions, drop tests and food-contact declarations.
Under differential scanning calorimetry performed per ISO 11357-3:2018, the crystallisation peak temperature typically falls between 112 °C and 118 °C at a cooling rate of 10 °C/min, while the melting peak temperature lies near 130 °C. These thermal transitions are relevant when setting mould temperatures and when predicting post-mould shrinkage.
| Property | Test method | Nominal value | Unit |
|---|---|---|---|
| Melt mass-flow rate | ISO 1133-1:2022 | 7.5 | g/10 min |
| Density | ISO 1183-1:2019 | 0.956 | g/cm³ |
| Tensile yield stress | ISO 527-2:2012 | 24–28 | MPa |
| Flexural modulus | ISO 178:2019 | 1,100 | MPa |
| Notched Izod impact strength, 23 °C | ISO 180/A:2023 | 4–6 | kJ/m² |
| Vicat softening temperature | ISO 306/A120 | 123 | °C |
FI0750 is typically supplied as pelletised resin in 25 kg bags or bulk containers. The pellet geometry is compatible with gravimetric blenders and desiccant dryers. Because the grade is a high-density ethylene homopolymer, moisture uptake is low; however, surface condensation on cold pellets moved into a warm plant can introduce defects, and handling controls should maintain pellet temperature above dew point.
The differentiation is most visible in capillary rheometry. Extrusion-grade high-density polyethylene with a melt flow rate near 0.3 g/10 min exhibits a zero-shear viscosity roughly 25 times higher than FI0750 at the same 190 °C reference temperature. This elevated viscosity is required for bubble stability in blown film and parison hang strength in blow moulding, but it penalises injection-moulding cycle time through higher screw torque and longer plasticating time. FI0750 is formulated to shift the crossover point between viscous and elastic response toward higher shear rates; in practical terms, the material reaches an apparent viscosity below 100 Pa·s at a wall shear rate around 1,000 s⁻¹, whereas a fractional-melt blow-moulding grade can remain above 300 Pa·s under the same conditions. The consequence is faster filling at moderate injection pressures and lower sensitivity to flow hesitation in multi-cavity tools.
Die swell is another distinction. FI0750 melt exhibits lower extrudate swell than fractional-melt blow-moulding grades because the shorter average chain length and narrower molecular weight distribution limit elastic recovery at the die exit. This is advantageous in injection moulding because the melt does not expand as aggressively into thin ribs, but it reduces parison integrity if the material is mistakenly used in blow moulding. The grade is therefore not a drop-in for blow moulding operations that require a melt strength above 8 cN at 190 °C in a Rheotens test; published data for FI0750 in such configuration is limited.
| Variable | FI0750 | Representative HDPE blow moulding grade | Representative HDPE film grade |
|---|---|---|---|
| Melt mass-flow rate at 190 °C/2.16 kg | 7.5 g/10 min | 0.25–0.35 g/10 min | 0.5–0.8 g/10 min |
| Density | 0.956 g/cm³ | 0.948–0.952 g/cm³ | 0.950–0.954 g/cm³ |
| Tensile yield stress | 24–28 MPa | 20–24 MPa | 20–24 MPa |
| Flexural modulus | 1,100 MPa | 850–950 MPa | 900–1,000 MPa |
| Typical melt temperature | 200–240 °C | 170–200 °C | 190–220 °C |
| Primary processing technology | Injection moulding | Extrusion blow moulding | Blown film extrusion |
The values in the table are representative published ranges for general-purpose grades and should not be read as batch-certificate data. The separation between processing categories is governed primarily by melt flow rate and die swell, not by density alone; density differences of 0.004–0.008 g/cm³ alter stiffness and creep resistance by only a few percent in short-term loading.
For thin-wall crates and caps, the recommended melt temperature window for FI0750 is 200 °C to 240 °C. Barrel profile from feed to nozzle is typically set as 180–190 °C, 200–220 °C, 210–230 °C and 205–225 °C on a 45 mm diameter screw with L/D 22:1. Mould temperature is maintained between 10 °C and 40 °C with turbulent flow in cooling channels. Injection pressure at the screw tip is normally 80–120 MPa, with a holding pressure of 60–80 MPa applied for 4–8 s depending on part mass. Back pressure is set to 5–10 MPa to control melt density without excessive shear heating. Screw speed is limited to 80–120 rpm to avoid local temperatures exceeding 240 °C at the non-return valve.
Runner and gate sizing for FI0750 follows the same pressure-drop principles as other medium-flow HDPE injection grades. Cold runner diameters below 4 mm can cause premature freeze-off in thick sections because the high crystallisation temperature reduces the duration of the molten core. For rectangular edge gates, a gate depth of 60–75 % of the adjacent wall thickness is common, with land length no greater than 1.0 mm. Hot runner drops should be independently controlled, and tip temperature should be held below 250 °C to prevent resin degradation in the manifold.
On production machines with clamp force 1,800 tonnes and shot weight exceeding 5 kg, the limiting factor is not plastication capacity but cooling time in thick bosses. Crystallisation of HDPE proceeds rapidly once the mould wall drops below 90 °C; short-cycle settings below 20 s can produce post-mould shrinkage of 2.0–2.5 % in the flow direction and 1.5–2.0 % transverse, which must be compensated in tool dimensions. Differential shrinkage in ribbed areas can exceed 0.5 % and cause warpage if the mould uses non-uniform cooling. These field-level shrinkage bands are more informative than generic published shrinkage values for unfilled PE.
Batch-to-batch variation in melt flow rate is typically controlled within ±0.5 g/10 min on certificate of analysis. Because MFR alone does not fully describe molecular weight distribution, converters using closed-loop process control should monitor fill time, cushion position and screw recovery time as indirect rheological indicators. A shortening fill time at constant pressure often indicates slightly lower viscosity from a higher MFR lot; an increase in recovery time at fixed screw speed can indicate lower melt index or feed-zone bridging.
Drying is generally unnecessary when pellets are stored in sealed hoppers at ambient relative humidity below 60 %. At higher humidity, surface moisture can generate splay and strand bubbles; a predrying step of 2 h at 80 °C in a desiccant dryer with dew point below -30 °C is recommended. The product should not be processed above 260 °C or held in the barrel for more than 10 min, because thermal-oxidative chain scission can reduce molecular weight and toughness. Avoid mixing with polypropylene, polycarbonate or PET regrind unless the converter has determined compatibility under ISO 1133-1:2022 viscosity testing.
Cap and closure moulds running FI0750 require gate diameters at least 0.8 mm per 0.5 g shot mass for annular tunnel gating. On a 32-cavity hot runner mould with 0.6 mm valve gates, filling imbalance exceeded 3 % when the hot runner manifold was not thermally decoupled; the resulting short shots were eliminated by increasing manifold tip temperature to 220 °C and maintaining nozzle contact force above 15 kN. This is consistent with the shear-thinning behaviour measured under ISO 11443 capillary rheometry.
Venting depth for HDPE is typically 0.015–0.03 mm; deeper vents can flash at the low viscosity developed under high shear. Vent grooves should be placed at the end of fill and at knit lines. In multi-cavity closure moulds, a mould temperature gradient of more than 5 °C between the gate side and the cavity end can produce measurable warpage after ejection.
In applications where a polypropylene impact copolymer with a melt flow rate of 10–15 g/10 min is replaced by FI0750, the most significant change is the increase in density from roughly 0.900 g/cm³ to 0.956 g/cm³, requiring a part mass increase of approximately 6 % for identical volume. The trade-off is a substantially higher flexural modulus; FI0750 typically provides 1,100 MPa compared with 900–1,000 MPa for a representative impact copolymer, improving top-load and stack performance at equal wall stock. The melt flow rate of FI0750 is lower than many PP impact copolymers, so injection speed and runner diameters may require adjustment to prevent flow-front hesitation. Linear mould shrinkage is also higher: post-mould shrinkage can reach 2.0–2.5 % in the flow direction for FI0750, whereas the PP copolymer typically shrinks 1.2–1.8 %; tooling cut for PP will not be dimensionally interchangeable without recut or process compensation.
Low-temperature performance differs by geometry. The notched Izod impact of the PP impact copolymer is often above 10 kJ/m² at 23 °C and may remain ductile at -20 °C, while FI0750 at 23 °C falls in the 4–6 kJ/m² range. For un-notched drop impact, high-density polyethylene can behave in a ductile manner at low temperatures, but published data for this specific comparison is limited. Converters should not transfer PP low-temperature impact assumptions to FI0750 without specimen-level testing under ISO 179-1:2020 or ISO 180/A:2023.
The Vicat softening temperature of FI0750 near 123 °C under ISO 306/A120 is lower than the melting peak; PP copolymers can exhibit higher heat deflection temperatures in filled systems, but unfilled PP heat distortion temperatures under load are often lower than HDPE. The service temperature limit for FI0750 in structural applications should be established by creep testing under load, not by Vicat alone. Under ISO 899-1:2003 tensile creep testing, HDPE grades with similar density show increasing creep compliance above 50 °C; this is a controlling variable in tote boxes stored in warm warehouses or exposed to direct sunlight.
The environmental stress-crack resistance of FI0750 is not specified in the main injection-moulding bulletin; if the moulded article contacts detergents, surfactants or solvents, a parallel test under ASTM D1693 condition B or ISO 22088-1:2006 is required. Published data for this specific grade under all detergent chemistries is limited, so converters must evaluate stress-cracking on their part geometry rather than relying on neat-resin values.
For food-contact articles, Sinopec Fujian HDPE FI0750 may be assessed under FDA 21 CFR 177.1520 for olefin polymers and EU Regulation 10/2011 with overall migration limits of 10 mg/dm² for general food contact. The converter remains responsible for finished-article compliance, including organoleptic and migration testing. The grade is not intended for sustained-pressure piping; hydrostatic creep-rupture testing under ISO 9080 is outside the published product scope and published data for this specific configuration is limited.