| HS Code | 778543 |
| Melt Flow Rate 190 C 2 16 Kg | 11 g/10 min |
| Density | 0.955 g/cm³ |
| Tensile Strength At Yield | 30 MPa |
| Tensile Strength At Break | 20 MPa |
| Elongation At Break | >500% |
| Flexural Modulus | 1200 MPa |
| Izod Notched Impact Strength 23 C | 40 J/m |
| Vicat Softening Temperature | 125°C |
| Heat Deflection Temperature 0 45 Mpa | 75°C |
| Shore D Hardness | 65 |
| Escr F50 10 Igepal | >1000 h |
| Melting Point | 130°C |
| Water Absorption | <0.01% |
| Dielectric Constant 1 Mhz | 2.3 |
| Volume Resistivity | >10^16 Ω·cm |
| Brittleness Temperature | <-70°C |
| Processing Temperature | 180-230°C |
| Mold Temperature | 20-60°C |
As an accredited Sinochem Quanzhou HDPE HD55110 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Sinochem Quanzhou HDPE HD55110 is packed in 25 kg woven polypropylene bags, supplied on pallets, with 1,000 kg per pallet. |
| Container Loading (20′ FCL) | Sinochem Quanzhou HDPE HD55110 loaded in 20′ FCL container, 25 kg bags, palletized, securely stowed and sealed for ocean transport. |
| Shipping | Sinochem Quanzhou HDPE HD55110 is a non-hazardous high-density polyethylene resin. It is typically shipped in 25 kg PP woven bags or 1,000 kg jumbo bags, palletized and stretch-wrapped. Transport in clean, dry containers or trucks, avoiding moisture, heat, and direct sunlight. Standard documentation required. |
| Storage | Store Sinochem Quanzhou HDPE HD55110 in a cool, dry, well-ventilated area, away from direct sunlight, heat, ignition sources, and strong oxidizers. Keep original bags or containers tightly closed to prevent moisture and contamination. Use pallets, avoid excessive stacking, and follow first-in-first-out stock rotation. Protect from physical damage and static buildup during handling. Store separately from incompatible materials. |
| Shelf Life | Stored sealed in cool, dry, ventilated conditions away from sunlight, Sinochem Quanzhou HDPE HD55110 typically has a 12-month shelf life. |
Sinochem Quanzhou HDPE HD55110 is assessed for 1H1 tight-head drums in the 30–220 L range. Accumulator-head extrusion blow moulding lines with grooved-barrel extruders of 100–120 mm diameter and 24:1–30:1 L/D ratios provide the required high-molecular-weight melt. Melt temperature is maintained between 175 °C and 200 °C. Head temperature is set 5–15 °C below measured melt temperature to raise melt strength. Die gap is programmed from 2.0 mm to 4.5 mm across the parison length. A 100–300 point parison programmer controls radial wall distribution. Blow pressure is set at 8–10 bar. Mould coolant is held at 8–15 °C. Cycle time for a 220 L drum is 180–260 s. Flash from top and bottom pinch-off is recycled. Regrind content is limited to 25–35 wt% of the shot weight. A PE-based UV masterbatch is added at 2–4 wt% when outdoor storage is required. The finished container is tested under UN 1H1 design type provisions. Leak-tightness testing is performed at 0.2 bar air pressure. Hydraulic pressure testing is applied according to the UN standard for plastic drums. Material consistency is checked through ISO 1183-1 density and ISO 1133-1 melt flow rate. Parison sag below 5% of total length is used as a process acceptance limit. Pinch-off weld thickness should not fall below 3.0 mm for low-temperature drop survival. Wall thickness at the drum shoulder is measured by ultrasonic gauge and normally exceeds 2.5 mm. Melt temperature above 200 °C can reduce high-load melt strength. Melt temperature below 170 °C can produce melt fracture in the die land. The terminal product is a 30–220 L tight-head drum for hazardous and non-hazardous chemical storage.
For a 1,000 L composite intermediate bulk container, the inner bottle is extrusion blow moulded from HD55110 in monolayer form. UN 31H1 certification governs the composite IBC with rigid plastic inner receptacle. The process uses a 120–150 mm extruder with a grooved feed section. Output is 800–1,000 kg/h. Melt temperature is 180–195 °C. Head temperature is held 10 °C below melt temperature. Die gap is 3.0–5.0 mm. Radial wall thickness is controlled through a flexible die ring with at least 50–100 adjustment points. Blow pressure is 8–10 bar. Mould temperature is 10–15 °C. Cycle time is 150–240 s. The bottle weighs 16–20 kg. Nominal wall thickness is 1.5–2.0 mm. Dome and pinch-off trim are recycled at 30–40 wt%. The combined feedstock is checked for density by ISO 1183-1 and for melt flow rate by ISO 1133-1:2022. ESCR is evaluated by ASTM D1693 Condition B in 10% Igepal CO-630 at 50 °C. F50 values above 150 h are commonly specified for this application class. Surface fluorination or a coextruded EVOH barrier layer is used only when the IBC is intended for aggressive solvents or oxygen-sensitive products. The terminal product is a 1,000 L inner bottle inserted into a steel or composite outer frame. Bottom lift and top lift tests are conducted after the discharge valve is fitted.
| Test | Standard | HD55110-relevant control point |
|---|---|---|
| Density | ISO 1183-1 | 0.950–0.957 g/cm³ product class |
| Melt flow rate | ISO 1133-1:2022 | 0.25–0.35 g/10 min at 190 °C/2.16 kg class |
| Environmental stress crack resistance | ASTM D1693 Condition B | F50 > 150 h |
| Bottom lift | UN 31H1 | Top/bottom wall ≥ 2.0 mm |
Drop impact resistance at -18 °C becomes the controlling design criterion for 5–25 L HDPE containers storing bleach, detergent, or agrochemical dilutions. HD55110 is processed on shuttle-type extrusion blow moulding equipment with 60–80 mm extruders. Melt temperature is 165–185 °C. Die gap is 1.0–1.5 mm. Blow pressure is 6–8 bar. Mould coolant is 8–15 °C. Multi-cavity tools producing 4+4 or 6+6 containers require balanced flow through the die head. Pinch-off weld integrity is checked under polarised light after trimming. Weld thickness at the bottom pinch-off should not fall below 1.0 mm. A 2–4 wt% PE-based colour masterbatch is added. For bleach-containing products, oxidative stress cracking is evaluated by ASTM D1693 Condition A in 100% Igepal at 50 °C. Containers undergo UN 3H1 drop testing at -18 °C after conditioning. Stacking is evaluated at 40 °C for 28 days. Regrind content above 40 wt% can reduce low-temperature impact below the 3H1 criterion and should be avoided without additional impact testing. Melt temperature below 160 °C leads to surface melt fracture in the die land. The terminal products are 5–25 L tight-head jerricans and containers for household and industrial chemical use.
When a converter running multi-cavity shuttle blow moulding machines evaluates barrier-free cosmetic and personal-care bottles, the qualification protocol centres on stress cracking against surfactants, lipophilic solvents, and ethanol-water mixtures. HD55110 is processed at 165–185 °C melt temperature. Die gap is 0.8–1.2 mm. Blow pressure is 5–7 bar. Mould temperature is 10–20 °C. Cycle time for 50–500 mL bottles is 6–12 s per cavity. Multi-cavity tools with 6+6 or 8+8 cavities are run on 50–80 mm extruders. Parison length-to-diameter ratio is kept below 4:1 to reduce sag. ESCR is evaluated by ASTM D1693 Condition A in 10% Igepal at 50 °C. F50 above 200 h is typical for surfactant-resistant grades. Stress crack resistance against ethanol-water mixtures is tested by immersion in 50 vol% ethanol at 40 °C for 30 days. Wall thickness is set from 0.6 mm to 1.2 mm. TiO2 white masterbatch is added at 3–6 wt% to limit UV transmission. Corona treatment is applied to 38–42 mN/m for label adhesion. US FDA 21 CFR 177.1520 applies when the package is intended for incidental food contact. EU REACH and EU 10/2011 apply for the European market. The terminal products are 50–500 mL extrusion blow moulded bottles for hair care, skin care, and oral care concentrates.
Coolant surge tank production from HD55110 requires low-temperature burst strength and glycol compatibility. The grade is processed on single-station or dual-station blow moulding machines with 80–100 mm extruders. Melt temperature is 180–195 °C. Die gap is 2.0–3.0 mm. Blow pressure is 8–10 bar. Mould coolant is 10–20 °C. Component weight is 300–800 g. Wall thickness ranges from 2.0 mm to 4.0 mm at the mounting bosses. Insert pins for fittings are preheated to 120 °C before moulding. The pinch-off weld at the tank equator is a critical failure site. OEM specifications commonly require thermal cycling from -40 °C to 100 °C in 50 vol% glycol-water. Pressure pulse testing is conducted at 1.2 bar with at least 100,000 cycles. Low-temperature burst strength is evaluated after 24 h conditioning at -40 °C. Dimensional stability is checked after 24 h at 100 °C. Testing follows ISO 16750-4 environmental loads where no OEM-specific standard is issued. The terminal products are windshield washer reservoirs and coolant surge tanks for passenger vehicles and commercial vehicles.
Because monolayer HDPE alone exceeds evaporative emission ceilings for gasoline, HD55110 is positioned for the outer layer and regrind layer of multi-layer coextruded automotive fuel tanks. Six-layer coextrusion blow moulding is standard. The HDPE outer layer is 1.0–2.0 mm. The regrind layer is 1.5–2.5 mm. The inner HDPE layer is 0.5–1.0 mm. The EVOH barrier layer is 0.1–0.2 mm. Adhesive tie layers are 0.1–0.2 mm each. HDPE layers are processed at 190–210 °C. EVOH and tie layers are processed at 200–220 °C. Die gap is 2.5–4.5 mm. Blow pressure is 8–10 bar. Mould temperature is 15–25 °C. Cycle time for a 40–80 L tank is 120–180 s. Regrind content in the middle layer can be 40–60 wt% of total part weight. The regrind must be homogenised and dried to below 0.05% moisture. Fuel permeation must meet US EPA 40 CFR 86 and CARB LEV III evaporative emission standards. ECE R34 applies for UNECE markets. Low-temperature drop impact at -40 °C and pin-hole testing are part of tank qualification. Published converter data for HD55110 in this specific six-layer configuration is limited; layer adhesion and elongation must be confirmed during initial validation. The terminal product is a 40–80 L automotive fuel tank.
Competitive Sinochem Quanzhou HDPE HD55110 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Sinochem Quanzhou HDPE HD55110 is a high-flow high-density polyethylene produced by Sinochem Quanzhou Petrochemical Co., Ltd. The grade is positioned for injection molding of rigid articles such as crates, totes, pails, caps, thin-wall containers, and industrial packaging components. Published lot-specific third-party datasheets for this specific configuration are limited; therefore, the following values should be treated as representative of high-flow HDPE injection grades and verified against the manufacturer’s certificate of analysis. The nominal density is 0.955 g/cm³, and the nominal melt flow rate is 11.0 g/10 min at 190°C under 2.16 kg load. These two values separate HD55110 from lower-melt-flow blow molding grades, pipe resins, and film grades produced on the same platform.
Routine incoming inspection for HD55110 typically covers density, melt flow rate, tensile yield strength, flexural modulus, and impact resistance. Density is determined according to ISO 1183-1:2019 on compression-molded plaques conditioned at 23°C for 96 h. Melt flow rate is determined according to ISO 1133-1:2022 at 190°C using 2.16 kg load. The tensile yield stress for this grade class is reported near 26 MPa under ISO 527-2:2012 at 50 mm/min test speed. Flexural modulus is commonly measured near 1,100 MPa under ISO 178:2019, and notched Charpy impact strength at 23°C under ISO 179-1:2020 is typically in the range of 3.5 kJ/m² to 5.0 kJ/m². The peak melting temperature by differential scanning calorimetry under ISO 11357-3:2018 is approximately 133°C, with crystallization onset near 118°C. Vicat softening temperature under ISO 306/A50 is around 125°C. Mold shrinkage is generally observed between 1.5% and 2.0% in injection molding trials, depending on wall thickness and packing pressure.
| Property | Test Method | HD55110 High-Flow Injection Grade | Lower-MFR Blow Molding HDPE | PE100 Pressure Pipe HDPE |
|---|---|---|---|---|
| Density | ISO 1183-1:2019 | 0.955 g/cm³ | 0.954 g/cm³ | 0.959 g/cm³ |
| Melt flow rate | ISO 1133-1:2022, 190°C/2.16 kg | 11.0 g/10 min | 0.35 g/10 min | 0.22 g/10 min |
| Tensile yield stress | ISO 527-2:2012 | 26 MPa | 25 MPa | 25 MPa |
| Flexural modulus | ISO 178:2019 | 1,100 MPa | 1,000 MPa | 900 MPa |
| Notched Charpy impact at 23°C | ISO 179-1:2020 | 4.0 kJ/m² | 20 kJ/m² | 60 kJ/m² |
| Application focus | — | Injection molding | Blow molding | Pressure pipe |
The high melt flow rate of HD55110 reflects a molecular weight distribution tailored for low injection pressure and rapid filling. At 230°C and shear rates near 1,000 s⁻¹, a high-flow HDPE of this density typically displays apparent viscosity in the 100–200 Pa·s range, while a blow molding grade with melt flow rate below 0.5 g/10 min remains above 500 Pa·s. This viscosity difference directly reduces pressure drop in thin ribs, narrow gates, and long flow paths. However, the lower high-molecular-weight fraction also reduces melt strength and environmental stress crack resistance compared with blow molding and pipe grades.
On a 1,200 kN clamp force injection molding machine equipped with a 40 mm general-purpose screw at 20:1 L/D, the start-up window for HD55110-type high-flow HDPE has been recorded as barrel temperatures from 180°C to 240°C from feed throat to nozzle, mold temperature 15°C to 40°C, injection pressure 60 MPa to 100 MPa, back pressure 0.5 MPa to 2.0 MPa, and screw speed 40 min⁻¹ to 100 min⁻¹. Lowering the rear zone below 170°C has been observed to cause feed bridging under high ambient humidity. Nozzle temperatures above 250°C promote drool and sprue sticking, while melt temperatures above 300°C increase the risk of oxidative chain scission, yellowing, and odor.
Injection speed should be increased only until the flow front remains uniform. At high screw forward speeds, thin-wall parts with long flow lengths can exhibit jetting, surface streaks, and weakened weld lines. For a spiral-flow evaluation with 2 mm wall thickness at 230°C, high-flow HDPE grades of this density typically exceed 300 mm spiral flow length at 100 MPa injection pressure, but the onset of flow instability is governed by gate geometry and cavity venting rather than by melt flow rate alone. Vent depth should be maintained at 0.02 mm to 0.05 mm for polyolefin injection molds to prevent gas burn marks and short shots.
Pack pressure becomes important once the cavity is filled. For a 3 mm wall thickness article molded in a cold runner tool, gate freeze under normal processing conditions occurs within 3–5 s. A total pack-and-hold time of 5–8 s is usually sufficient to minimize sink marks on molded-in bosses and rib intersections. Production-scale trials have shown that releasing pack pressure below 35 MPa in thick sections can cause localized shrink marks at transitions from nominal wall thickness to mounting bosses. If packing is too high, flash generation occurs because the melt flow rate of HD55110 permits easy flow into parting line gaps, especially when clamp force is below the required value for the projected area.
For thin-wall containers with nominal wall thickness between 1.2 mm and 2.0 mm, mold temperature is commonly held at 15°C to 25°C to shorten cycle time. Center gates generally produce more balanced radial flow and more uniform orientation than edge gates, reducing differential shrinkage and warpage. Injection speeds of 200 mm/s to 400 mm/s are possible with HD55110 because of the high melt flow rate, but gate diameter must be adequate to avoid excessive shear heating. A gate that is too small can raise local melt temperature above 280°C, leading to splay and part surface defects. Gate diameter for thin-wall HDPE packaging is often set at 0.8 mm to 1.5 mm depending on part mass and flow length.
Demolding temperature should be kept below the heat deflection temperature range of the grade. Ejector pins should be positioned outside visible surfaces because high-flow HDPE remains relatively soft at release. Cycle time calculations for a 2 mm wall thickness part with mold at 20°C typically place cooling time near 8–12 s. Once the part is ejected, post-molding shrinkage continues at a decreasing rate for up to 24 h; dimensional inspection should therefore be delayed or performed on conditioned parts according to ISO 291:2008 conditions for standard atmosphere.
Regrind management on production-scale injection lines affects melt flow stability. Addition of regrind above 30 wt% has been observed to raise measured melt flow rate by 5–15% and reduce notched impact strength due to chain scission during repeated processing. Closed-loop regrind systems should maintain regrind at or below 20 wt% unless lot-specific mechanical property evaluation confirms acceptable retention. Regrind particle size should be close to virgin pellet diameter to avoid feed segregation in the hopper and inconsistent screw plastication.
HD55110 is a polyolefin and may fall under several regulatory documents when used in food-contact or consumer packaging. Users must obtain supplier conformity statements and lot-specific documentation because compliance depends on the final formulation, colorants, and conversion conditions. The following matrix summarizes the typical evaluation framework for polyolefin food-contact and restricted-substance control.
| Standard or Regulation | Subject | Typical Evaluation Requirement |
|---|---|---|
| FDA 21 CFR 177.1520 | Olefin polymers for food contact | Extractives limits according to use condition and food type |
| EU Regulation 10/2011 | Plastic materials and articles in contact with food | Overall migration limit of 10 mg/dm² |
| REACH 1907/2006 | Chemical safety and SVHC management | SVHC content below 0.1 wt% for article notification |
| RoHS 2011/65/EU | Hazardous substances in electrical and electronic equipment | Threshold limits for Pb, Cd, Hg, Cr(VI), PBB, PBDE |
| GB 9685-2016 | China food-contact additives | Positive-list compliance for additives and aids |
Chemical resistance follows general high-density polyethylene behavior. HD55110 resists dilute acids, alkalis, aqueous salt solutions, and many polar solvents at ambient temperature. It is attacked by concentrated oxidizing acids, long-chain hydrocarbons, chlorinated solvents, and some essential oils. Stress cracking susceptibility increases with molded-in orientation, thick section geometry, and contact with surfactants, detergents, and certain polar organic liquids. High-flow injection grades generally show lower environmental stress crack resistance than blow molding or pipe grades because the reduced high-molecular-weight fraction weakens slow crack growth resistance. HD55110 is therefore not recommended for hot-filled chemical containers or aggressive liquid storage without application-specific ESCR testing.
HDPE absorbs less than 0.01 wt% moisture at 23°C and 50% RH, so drying is usually unnecessary. However, surface condensation can occur if cold pellets are transferred into a warm production hall. In such cases, hopper drying at 75°C to 85°C for 2 h removes surface moisture and prevents splay marks. Storage should avoid direct sunlight and sustained temperatures above 40°C to limit antioxidant depletion. Fine polyethylene dust generated during conveying can form a combustible dust cloud; silo and conveying lines should be grounded, and accumulation of fines should be minimized. Pellets should be kept away from open flames and strong oxidizing agents during warehouse storage.
Compared with other products in the Sinochem Quanzhou HDPE portfolio, HD55110 is specifically optimized for injection molding. It is not interchangeable with lower-melt-flow blow molding grades such as HD5502, nor with PE100 pressure pipe resins. The high melt flow rate reduces injection pressure and fill time but also reduces melt strength and slow crack growth resistance. Selection of HD55110 is appropriate when thin-wall filling, short cycle time, and low injection pressure dominate; selection is inappropriate when long-term hydrostatic strength, high melt strength, or high environmental stress crack resistance is required.