| HS Code | 806281 |
| Glass Fiber Content | 30% |
| Density | 1.53 g/cm³ |
| Tensile Strength | 100 MPa |
| Tensile Elongation At Break | 2.0% |
| Flexural Strength | 155 MPa |
| Flexural Modulus | 8500 MPa |
| Notched Izod Impact Strength | 6 kJ/m² |
| Heat Deflection Temperature At 1 82 Mpa | 200 °C |
| Melting Point | 225 °C |
| Water Absorption | 0.03% |
| Molding Shrinkage | 0.2–0.5% |
| Flammability Rating | UL94 V-0 |
As an accredited Shinkong SHINITE® PBT+GF 3886 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Shinkong SHINITE® PBT+GF 3886 is packaged in 25 kg moisture-barrier bags, palletized for industrial shipping and storage. |
| Container Loading (20′ FCL) | Shinkong SHINITE® PBT+GF 3886 is loaded into a 20′ FCL, palletized in bags and securely stowed for export shipment. |
| Shipping | Shinkong SHINITE® PBT+GF 3886 is shipped as non-hazardous engineering plastic pellets in moisture-barrier bags or pails, palletized and stretch-wrapped. Store in a cool, dry, ventilated area away from direct sunlight and moisture. Handle according to local regulations; no special UN transport classification. |
| Storage | Store Shinkong SHINITE® PBT+GF 3886 in a cool, dry, well-ventilated area away from direct sunlight, heat, ignition sources, and moisture. Keep original containers tightly closed when not in use to prevent moisture absorption and contamination. Protect from physical damage and keep away from incompatible chemicals. Avoid prolonged storage in hot or humid conditions. Follow the manufacturer’s safety data sheet and local regulations. |
| Shelf Life | Shinkong SHINITE® PBT+GF 3886 has a typical shelf life of 24 months when stored dry, cool, and in original unopened packaging. |
Competitive Shinkong SHINITE® PBT+GF 3886 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Shinkong SHINITE® PBT+GF 3886 is a glass-fiber-reinforced polybutylene terephthalate injection-molding compound supplied by Shinkong Synthetic Fibers. The product designation 3886 is manufacturer-specific; in current supplier literature the grade is identified as a 30 wt% glass-fiber-reinforced PBT formulation, though the lot certificate remains the controlling document for the exact glass content, additive package, and viscosity. The material is intended for injection-molded components that require higher dimensional stability, heat resistance, and creep resistance than unfilled PBT can provide. It is commonly specified in electrical connectors, relay housings, coil bobbins, cooling fan brackets, and automotive underhood sensor housings. Because PBT crystallizes rapidly and absorbs less moisture than polyamide-based alternatives, the compound suits high-cycle molding and applications where electrical properties must remain stable under humid conditions. However, the glass-fiber reinforcement introduces anisotropic shrinkage, weld-line sensitivity, and a requirement for controlled drying before melt processing.
The property envelope below is representative of commercial 30 wt% glass-fiber-reinforced PBT injection-molding compounds and is not a substitute for the current Shinkong lot certificate. Values are sensitive to fiber-length retention, mold orientation, and conditioning history. Mechanical tests are typically conducted at 23 °C after conditioning at 50 % RH unless another condition is indicated.
| Property | Test method | Typical range |
|---|---|---|
| Density | ISO 1183-1:2019 | 1.50–1.60 g/cm³ |
| Tensile strength at break | ISO 527-2:2012 | 110–140 MPa |
| Tensile modulus | ISO 527-2:2012 | 9,000–11,000 MPa |
| Flexural strength | ISO 178:2019 | 160–200 MPa |
| Flexural modulus | ISO 178:2019 | 8,000–10,000 MPa |
| Charpy notched impact strength | ISO 179-1:2023 | 7–12 kJ/m² |
| Heat deflection temperature, 1.8 MPa | ISO 75-2:2013 | 195–215 °C |
| Mold shrinkage, injection direction | ISO 294-4:2018 | 0.2–0.6 % |
| Mold shrinkage, transverse direction | ISO 294-4:2018 | 0.6–1.2 % |
The difference between injection-direction and transverse shrinkage is a direct consequence of fiber orientation. In plate-like geometries, the shrinkage differential can exceed 0.4 %, and flat parts with nonuniform wall thickness may warp unless mold cooling, gate placement, and ejection timing are matched to the orientation field.
Pre-drying is mandatory before injection molding. The pellets should be dried in a desiccant dryer with a dew point at or below -30 °C and a hot-air temperature of 120 °C for 4–6 h. The residual moisture target is ≤ 0.02 wt%. PBT undergoes hydrolytic chain scission in the melt; moisture above this threshold can produce surface splay, reduced molecular weight, and brittle parts even when the machine parameters are otherwise acceptable. Barrel temperature settings for the melt phase should generally be held between 235 °C and 250 °C at the nozzle, with rear zones between 220 °C and 235 °C. Mold temperature should be maintained between 80 °C and 110 °C to promote sufficient crystallinity and to stabilize as-molded dimensions. At mold temperatures below 80 °C, the heat deflection temperature of the formed part may fall and post-mold dimensional change increases. Above 110 °C, cycle time lengthens without a proportional gain in mechanical performance for most part geometries. Injection speed for general-purpose parts is usually set between 50 and 150 mm/s; thin-wall sections below 1.0 mm may require injection speeds above 200 mm/s. On 120–180 t electric injection molding machines processing similar glass-fiber-reinforced PBT grades, retaining a cushion of 2–4 mm and keeping screw speed below 120 rpm are common industrial settings. Excessive screw speed increases fiber breakage and can lower tensile strength by 5–10 % due to loss of fiber aspect ratio.
Fiber orientation at knit lines follows the meeting flow front; the glass fibers do not re-entangle across the interface. Consequently, weld-line tensile strength in glass-fiber-reinforced PBT can be 40–60 % lower than the bulk flow-direction value. This limitation controls part design more than the nominal datasheet strength value. Gate positions should be selected so that knit lines are placed away from snap-fit hooks, self-tapping screw bosses, and thin structural ribs. In cold-runner two-plate molds, sequential valve gating or cavity pressure transducers can be used to hold a uniform melt-front velocity and reduce adverse knit-line formation. For sections thinner than 1.2 mm, a continuous flow length-to-thickness ratio above 200:1 may produce short shots if the melt volume-flow rate of the lot sits at the lower end of the supplier control window. When the mold contains multiple cavities with unequal runner lengths, shot-to-shot consistency improves by balancing the runner system to within 5–10 % of the highest cavity pressure.
At continuous service temperatures above 80 °C in humid environments, hydrolysis of the PBT ester linkages becomes the primary degradation pathway. Exposed glass fibers at the part surface can accelerate moisture wicking into the polymer matrix. Combined stress and hot-water exposure can induce environmental stress cracking, particularly around molded-in metallic inserts or sharp internal corners. The material is not recommended for immersion in hot water above 80 °C unless the specific lot has passed a supplier-defined long-term hydrolysis test. Resistance to aliphatic hydrocarbons, mineral oils, and dilute acids at room temperature is generally adequate, but strong oxidizing acids, hot alkaline solutions, and chlorinated solvents under stress should be avoided. Prolonged exposure to hot oil above 120 °C may extract low-molecular-weight additives and alter the surface crystalline structure, causing dimensional instability and loss of appearance.
Unfilled PBT has a heat deflection temperature at 1.8 MPa of approximately 50–60 °C. The 30 wt% glass-fiber-reinforced PBT class raises this value to 195–215 °C, allowing the 3886 grade to tolerate short-term soldering heat, connector terminal retention, and underhood radiant heat that would distort unmodified PBT. The trade-off is that the glass-filled product has lower melt flow and requires higher injection pressure, and the anisotropic shrinkage demands more deliberate mold design.
Compared with a 30 wt% glass-fiber-reinforced polyamide 66, the PBT product absorbs less moisture at equilibrium. At 23 °C/50 % RH, PBT-GF30 typically reaches 0.1–0.5 wt% moisture, while PA66-GF30 typically reaches 1.5–3.0 wt%. This gives PBT more stable dielectric properties and less dimensional movement under humidity change. However, the notched Charpy impact of PBT-GF30 at 23 °C is generally 7–12 kJ/m², whereas PA66-GF30 can reach 10–15 kJ/m². At low temperature, the impact difference becomes more pronounced. The heat deflection temperature at 1.8 MPa for PBT-GF30 is typically 40–50 °C lower than that of PA66-GF30, which restricts use in hot engine brackets, gear housings, and bearing carriers where polyamide-based grades are preferred.
| Comparison axis | PBT+GF 3886 class | PA66-GF30 | PPS-GF40 |
|---|---|---|---|
| Equilibrium moisture at 23 °C/50 % RH | 0.1–0.5 wt% | 1.5–3.0 wt% | ≤ 0.1 wt% |
| Heat deflection temperature, 1.8 MPa | 195–215 °C | 245–260 °C | ≥ 260 °C |
| Typical melt processing temperature | 235–250 °C | 270–300 °C | 300–340 °C |
Against a 40 wt% glass-fiber-reinforced polyphenylene sulfide, the PBT product processes at lower melt temperatures and does not require mold temperatures above 135 °C. PBT-GF30 can therefore be molded on conventional water-heated tooling. However, chemical resistance to hot oil, strong organic acids, and continuous-use temperatures above 180 °C is inferior to PPS-GF40. The 3886 grade should not be specified for aggressive chemical-processing components or high-temperature underhood zones without validation.
Compliance with RoHS Directive 2011/65/EU and REACH Regulation (EC) No 1907/2006 must be documented by the supplier for each shipment. The base glass-fiber-reinforced PBT compound is generally supplied as cylindrical pellets. Storage should occur in closed containers at 5–40 °C. If containers remain open for more than 24 h at ambient humidity, the material should be re-dried before processing. Melt temperatures above 260 °C or residence times exceeding 5 min can liberate volatile decomposition products and should be avoided. Published data for this specific configuration is limited where the 3886 suffix does not appear on the supplier’s current public datasheet; therefore, all design decisions should be validated against the lot certificate and the end-use application requirements.