| HS Code | 867204 |
| Product Name | Shanxi PCEC HDPE DMDA8920 |
| Polymer Type | High Density Polyethylene |
| Density | 0.954 g/cm³ |
| Melt Flow Rate | 0.9 g/10 min |
| Melting Point | 130 °C |
| Vicat Softening Point | 120 °C |
| Tensile Strength At Yield | 25 MPa |
| Tensile Strength At Break | 35 MPa |
| Elongation At Break | 600% |
| Flexural Modulus | 1100 MPa |
| Izod Impact Strength | 80 J/m |
| Hardness | 60 Shore D |
| Environmental Stress Crack Resistance | >1000 h |
| Heat Deflection Temperature | 75 °C |
| Brittleness Temperature | -70 °C |
| Water Absorption | <0.01% |
| Dielectric Constant | 2.3 |
| Volume Resistivity | >10^16 Ω·cm |
As an accredited Shanxi PCEC HDPE DMDA8920 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Shanxi PCEC HDPE DMDA8920 typically comes in 25 kg PP woven bags, also available in 1,000 kg jumbo bags. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with Shanxi PCEC HDPE DMDA8920 resin in 25kg bags, palletized, shrink-wrapped, and securely stowed for export. |
| Shipping | For Shanxi PCEC HDPE DMDA8920, ship as non-hazardous polyethylene resin pellets in 25 kg bags, jumbo bags, or bulk containers. Keep dry, cool, ventilated, away from sunlight, heat, and ignition sources. Use covered transport; protect from moisture and contamination. No dangerous goods placards required; follow local regulations. |
| Storage | Store Shanxi PCEC HDPE DMDA8920 in a cool, dry, well-ventilated warehouse at ambient temperature, away from direct sunlight, heat, sparks, and flames. Keep original bags sealed, palletized, and off the floor. Avoid moisture, oils, acids, bases, oxidizers, and contaminants. Observe stacking limits to prevent deformation. Use clean handling equipment and prevent static buildup. Inspect packaging regularly. |
| Shelf Life | Shelf life is typically 24 months when stored unopened in original packaging, cool, dry, ventilated, away from sunlight and moisture. |
Shanxi PCEC HDPE DMDA8920 is a high-molecular-weight high-density polyethylene processed on extrusion blow-molding lines where parison melt strength, environmental stress crack resistance, and wall-thickness reproducibility determine downstream container service life. Typical conversion equipment includes grooved-feed extruders with length-to-diameter ratios between 24:1 and 30:1, melt temperatures between 185 °C and 205 °C, and mold temperatures between 10 °C and 20 °C. The application scenarios below define regulatory frameworks, regrind-addition boundaries, production-scale process configurations, and terminal article types for this specific grade.
On single-station accumulator blow-molding machines converted to 200 L tight-head chemical drums, Shanxi PCEC HDPE DMDA8920 is run as a virgin base with up to 25 wt% same-grade post-industrial regrind. The applicable dangerous-goods packaging framework is UN Model Regulations Chapter 6.1 for 1H1 closed-head plastics drums; a common marking is UN 1H1/Y1.8/250 for Packing Group II liquids with a maximum relative density of 1.8 and hydrostatic test pressure of 250 kPa. ISO 16101 plastics compatibility testing is applied to the filled inner surface before product qualification. Formulation ratio: 73–78 wt% virgin DMDA8920, 20–25 wt% same-grade regrind, and 2.0–2.5 wt% carbon black masterbatch for ultraviolet opacity. The process uses a 240–280 mm accumulator die head with 10–20 parison programming points to offset parison sag; melt temperature is held at 190–205 °C; blow-air pressure is 0.5–0.8 MPa; mold temperature is 12–20 °C; cooling time ranges from 160 s to 240 s because the bottom pinch-off weld and top shoulder remain the slowest cooling zones. Terminal product: 200 L tight-head chemical drums for export liquid chemicals, paints, agrochemical intermediates, and solvents compatible with high-density polyethylene. Operational boundary: aggressive oxidizing acids above 30% concentration and aromatic solvent blends require ISO 16101 barrier verification or fluorination treatment; regrind above 25 wt% reduces notched Izod impact after drop tests at -18 °C under ASTM D256.
Early-stage qualification of 1000 L rigid plastics inner receptacles under UN 31H2 requires confirmation that regrind inclusion does not depress environmental stress crack resistance below the threshold needed for stacking and hydraulic pressure testing. A 1000 L IBC inner bottle with at least 2.5 mm nominal wall thickness at the lower corners is produced from 70–80 wt% virgin DMDA8920 and 20–30 wt% same-grade regrind; foreign recycled HDPE is not introduced. ESCR is checked to ASTM D1693 condition B, 100% Igepal CO-630, F50, and acceptance is typically set at ≥100 h for the 30 wt% regrind compound, though published data for this specific configuration is limited and should be verified per lot. The downstream process is high-tonnage accumulator blow molding with shot capacities of 4.0–6.0 kg, a 180–260 mm parison programmer, wall-thickness profiles of 4–8 mm at corner transitions, and two-stage post-cooling with internal air circulation for 180–300 s. Terminal product: 1000 L composite IBC inner containers for UN 31H2/Y1.8/2000 transport of lubricants, water-based process chemicals, and food-approved intermediates. Compliance standards include ADR/RID Chapter 6.5, ISO 16101 chemical compatibility, and ASTM D1998 for tank-wall creep resistance. Limitation: regrind above 30 wt% produces disproportionate loss in top-load creep and sidewall bulge at 40 °C.
| Application segment | Regulatory and product standards | Critical test method | Typical acceptance criterion |
|---|---|---|---|
| 200 L tight-head drums | UN Model Regulations Chapter 6.1; UN 1H1/Y1.8/250 | ISO 16101 | No cracking after 28-day stack at 40 °C |
| 1000 L IBC inner bottles | ADR 6.5; UN 31H2/Y1.8/2000 | ASTM D1693 | F50 ≥100 h |
| 20–25 L jerry cans | UN 3H1/Y2.4/100 | UN drop test 1.2 m at -18 °C | No rupture |
| Agricultural sprayer tanks | EN 13575 | ASTM D638 | Yield stress ≥22 MPa |
| Multi-layer solvent containers | UN 1H1 / UN 3H1 | ASTM D3985 | OTR <5 cm³/(m²·day) |
| Automotive fluid reservoirs | ISO 22241-1 | ASTM D1693 | F50 ≥100 h |
Because multi-cavity shuttle extrusion blow molding of 20–25 L UN jerry cans runs with dual parisons and shorter residence times, stabilizer and masterbatch distribution becomes the principal quality variable. The process uses two- or four-cavity molds, melt temperatures of 185–205 °C, die temperatures of 190–210 °C, blow pressure of 0.5–0.7 MPa, mold temperature of 10–15 °C, and cycle times between 45 s and 70 s. Formulation ratio: 75–80 wt% virgin DMDA8920, 20–25 wt% same-grade regrind, 1.5–2.5 wt% UV-stabilized color masterbatch, and for outdoor service an additional 0.2–0.4 wt% hindered amine light stabilizer concentrate. Compliance for petroleum-derived or agrochemical fills uses UN 3H1/Y2.4/100 type testing for Packing Group II, and colorant selection requires migration testing under the UN 3H1 regime. Terminal product: 20–25 L tight-head jerry cans for lubricants, crop-protection chemicals, detergents, and water-based industrial intermediates. Operational boundary: regrind from containers previously used for hydrocarbons must be segregated and not used for oxidizing liquids; extrusion back pressure above 25 MPa at the die entry indicates over-gelled regrind.
Blow-molded high-density polyethylene tanks for tractor-mounted or trailed agricultural sprayers, typically in the 250–1000 L size class, place a different demand set on DMDA8920: the parison is longer, the pinch-off weld is longer, and the outer surface may be exposed to UV for 1500–3000 h per year. Formulation ratio for outdoor tanks: 96.5–97.5 wt% DMDA8920, 2.0–2.5 wt% carbon black masterbatch, and 0.5–1.0 wt% UV stabilizer concentrate, with post-industrial regrind capped at 15 wt% because long-parison processing loses wall-thickness control above this level. Process: single-head accumulator machine with shot capacity of 20–40 kg, die diameter of 350–500 mm, parison programming with 30–40 control points, blow pressure of 0.6–0.9 MPa, mold temperature of 8–15 °C, and cooling time of 300–600 s depending on nominal capacity. Compliance includes EN 13575 for static thermoplastic tanks for above-ground storage of chemicals, ISO 1183 for density verification, and ASTM D638 for tensile yield acceptance at not less than 22 MPa. Terminal product: 250–1000 L agricultural sprayer tanks and mobile chemical storage tanks. Limitation: opaque black tanks made only with recycled HDPE are not recommended; weld-line thickness below 70% of sidewall thickness after trimming is a rejection criterion.
For barrier containers used with methyl esters, toluene, or low-molecular-weight aromatics, monolayer DMDA8920 is inserted as the load-bearing outer layer of a six-layer coextrusion structure. Layer mass distribution: 75–80 wt% DMDA8920, 2–4 wt% ethylene-vinyl alcohol copolymer, 1–2 wt% maleated HDPE tie resin, and 15–20 wt% same-grade regrind core. The converter runs a six-layer coextrusion blow-molding head at 190–210 °C for HDPE layers and 200–210 °C for EVOH, with blow pressure of 0.6–0.8 MPa and mold temperature of 10–18 °C. Compliance for dangerous goods packed in such containers follows UN 1H1 or UN 3H1 marking under UN Model Regulations Chapter 6.1; barrier property testing uses ASTM D3985 for oxygen transmission at 23 °C and 0% RH, with a target oxygen transmission below 5 cm³/(m²·day) for the finished container. Terminal product: 5–20 L multi-layer bottles and jerry cans for agricultural solvents, crop-protection formulations, and volatile liquid chemicals. Process boundary: layer collapse or waviness occurs when HDPE melt temperature exceeds 210 °C because EVOH viscosity mismatch increases; shutdown requires purging with a 0.2 g/10 min class HDPE. Limitation: EVOH moisture pickup above 0.3% during processing creates gel streaks and interlayer delamination.
Automotive fluid reservoirs for diesel exhaust fluid and windshield washer fluid are blow molded in twin-station shuttle lines from DMDA8920 because combined environmental stress crack resistance and low-temperature impact are required by underhood thermal cycling. Formulation ratio: 80 wt% virgin DMDA8920, 20 wt% same-grade regrind, and 2.0 wt% carbon black or heat-stabilized masterbatch; copper-based colorants are not added because copper ions catalyze degradation of HDPE and DEF solutions. Process: twin-station shuttle machine with 10–20 kg shot, two-cavity tools, parison programmer set to 12–20 points, melt temperature of 185–200 °C, blow pressure of 0.5–0.7 MPa, cooling time of 80–140 s; leak testing is performed by pressure decay at 30–50 kPa after trimming. Compliance includes ISO 22241-1:2019 for diesel exhaust fluid handling materials and ASTM D1693 for ESCR. Terminal product: 10–40 L diesel exhaust fluid tanks, windshield washer reservoirs, and coolant expansion tanks. Operational boundary: molded-in brass inserts or non-HDPE welding nipples produce notch initiation sites; post-molded vibration welding must use 0.3–0.5 mm collapse depth and must not exceed 230 °C interface temperature to avoid thermal degradation.
Competitive Shanxi PCEC HDPE DMDA8920 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Shanxi PCEC HDPE DMDA8920 is a high-density polyethylene extrusion blow moulding resin aimed at large-volume, thick-walled industrial containers and vehicle fluid-management components. The grade is supplied as natural pellets and typically exhibits a density of 0.954 g/cm³ when determined under ISO 1183-1 and a melt mass-flow rate of 0.20 g/10 min at 190 °C under a 2.16 kg load when tested to ISO 1133-1. The low flow value corresponds to a high molecular weight fraction that raises melt strength and resistance to parison sag relative to injection-moulding grades with flow rates above 4 g/10 min. Typical tensile yield stress is reported near 25 MPa using ISO 527-2, elongation at break exceeds 500%, and flexural modulus is approximately 1,100 MPa using ISO 178. Environmental stress-cracking resistance under ASTM D1693, condition A, is normally stated as greater than 100 h in 100% Igepal CO-630 at 50 °C. These values are supplier-typical characterizations rather than guaranteed lot-release limits, and published data for high-temperature fuel-contact conditioning of the specific Shanxi PCEC formulation remains limited.
The product finds use in 30 L to 220 L open-head and tight-head drums, agricultural spray tanks, automotive diesel and fuel system components, and intermediate bulk container liners. In these applications, the grade is selected less for short-term stiffness than for resistance to environmental stress cracking caused by contact with detergents, crop-protection formulations, and hydrocarbon mixtures. Finished-part qualification normally includes hydraulic pressure testing, drop testing at low temperature, and stack-load testing at elevated temperature. Because DMDA8920 is a natural resin, ultraviolet stabilization and pigmentation must be added by the converter for long-term outdoor exposure.
The primary differentiation from lower-cost HDPE grades used for thin-walled household bottles appears in the balance between melt flow rate and molecular weight distribution. A commodity high-flow blow moulding resin may show a melt flow rate of 0.3–0.7 g/10 min at 190 °C under 2.16 kg, reducing extrusion torque and allowing faster cycles on small shuttle machines. DMDA8920 operates below 0.25 g/10 min, which increases screw back-pressure and energy input but gives the formed parison a longer hang time before diameter attenuation becomes uncontrollable. On accumulator-head equipment, the practical consequence is a reduction in top-to-bottom wall thickness variation when parison programming is set with a die gap opening progressively narrowed during extrusion.
The difference in environmental stress-cracking resistance is also significant where containers are exposed to surfactants, white oils, or agri-chemical concentrates. Grades with density above 0.960 g/cm³ may provide higher stiffness but typically show a more rapid failure under ASTM D1693 conditions because fewer tie molecules connect crystalline lamellae. DMDA8920’s reported density of 0.954 g/cm³ and high molecular weight support a more ductile response in the presence of polar stress-cracking fluids. The trade-off is in modulus; the material does not achieve the 1.4–1.6 GPa flexural modulus of highly crystalline injection resins, and this limits its replacement of engineered polyolefins where creep resistance under continuous load exceeds 40 MPa.
In blow moulding resins, density is not the sole predictor of long-term crack resistance. A high-density grade with density above 0.960 g/cm³ such as HDPE 5000S may show higher top-load strength and shorter cycle times, but it does not typically give the same stress-cracking resistance when containers store ethoxylated surfactant solutions or kerosene-based formulations. Conversely, a bimodal pipe resin with melt flow rate below 0.10 g/10 min has excellent slow crack growth resistance but is difficult to process on accumulator blow moulding because of very high extrusion torque and low drawability. DMDA8920 is therefore positioned as an intermediate molecular architecture: the flow rate permits an acceptable fill speed, while density and molecular weight distribution are balanced toward ESCR rather than maximum hardness.
Molecular architecture data for DMDA8920 indicate a broad multimodal molecular weight distribution typical of high molecular weight blow moulding resins. The low melt index alone does not describe parison behaviour; dynamic oscillatory rheometry at 190 °C shows a shear-thinning profile with a crossover frequency that is shifted lower relative to a monomodal resin of equivalent density. This broadening influences die swell, melt tear at the die lip, and pinch-off weld strength. Published viscosity curves for the exact Shanxi PCEC grade are not always supplied in distributor literature; when these data are absent, the use of capillary rheometry at 210 °C, 220 °C, and 230 °C is required before designing accumulator-head tooling.
Relative to high-flow injection HDPE with a melt flow rate of 8–20 g/10 min, DMDA8920 shows lower crystallinity and slightly lower tensile yield stress but much higher ESCR and melt strength. This makes it unsuitable for thin-wall injection moulding of caps and crates where cycle times below 20 s are required. Conversely, relative to a blow moulding HDPE with melt flow rate of 0.5–1.0 g/10 min, DMDA8920 may require longer cooling and higher clamp tonnage, but the resulting large-part container has fewer sidewall thin spots when the parison is dropped over long distances.
Extrusion blow moulding of large closed-head drums and intermediate bulk container liners with DMDA8920 is constrained by the interaction of melt temperature, die swell, and clamp force. The melt temperature is typically maintained between 190 °C and 220 °C; below 190 °C, the material can produce incomplete pinch-off fusion at the bottom weld, and above 220 °C, long parison hang times may lead to excessive sag on shot volumes above 15 L. Accumulator-head machines with shot capacity of 30–50 kg and clamp force of 800–1,200 kN are common for 200 L tight-head drums, although machine selection must be verified against the actual part mass and the required cooling time.
Tooling design affects the grade’s performance more than with lower molecular weight HDPE. Divergent die gaps of 1.5–2.5 mm at the lip, combined with parison programming over 10–30 discrete points, allow redistribution of wall thickness from the top pinch-off to the lower body. Failures observed on production-scale accumulator machines include local thinning at the shoulder transition when programming is too aggressive, and surface melt fracture when the die head is operated below 180 °C or with excessive line speed. Pinch-off weld integrity is evaluated by drop testing filled drums to UN 6.1.5 protocols or by sectioning the weld and measuring notched impact strength under ISO 179-1/1eA. A weld that passes hydrostatic testing may still fail at low temperature if the pinch-off zone retains polyethylene degradation products from prolonged residence time at high head temperature.
For tight-head drum tooling, the flash pocket depth and pinch-off insert geometry control weld quality. A pinch-off land width of 3–6 mm and an included angle of 30–45° are common starting points for high molecular weight HDPE. If the land is too wide, the weld zone remains thick and becomes the dominant impact failure site; if too narrow, the weld may cool before molecular interdiffusion completes. Flash trimming must be delayed until the part temperature drops below 60 °C, because molten HDPE flash above this temperature can carry away weld material and create a notch at the container base.
Cooling cycle management is a further processing boundary. For thick-walled liners with nominal wall thickness above 5 mm, internal air pressure of 0.6–0.8 MPa and blow time of 180–300 s are frequently required to prevent post-mould shrinkage and to maintain dimensional stability. Published data for this specific configuration is limited; cooling time must be derived from heat-transfer calculations using a mould temperature near 10–20 °C and verified by dimensional inspection after 24 h of conditioning at 23 °C.
Batch-to-batch viscosity variation in DMDA8920 is most readily observed on the blow moulding shop floor as a change in parison hang length and die swell at constant extruder settings. A lot with a slightly higher molecular weight fraction can generate higher back-pressure and require a 2–5 °C increase in barrel temperature to maintain the same screw speed. When the parison length at a given drop time changes by more than 5% between lots, the die programming should be re-validated; a compensator adjustment at the die gap without confirming the pinch-off weld can produce containers that pass visual inspection but fail low-temperature drop testing.
Because DMDA8920 operates at a low melt flow rate, screw configurations optimized for HDPE grades with melt flow rates above 0.35 g/10 min can generate excessive melt temperature at moderate screw speed. Single-screw extruders with 24:1 to 30:1 L/D and barrier-type mixing sections are generally suitable when screw speed is limited to 20–60 min⁻¹ and back-pressure is held below 15 MPa. Higher throughput rates in accumulator blow moulding require grooved-feed sections that improve conveying but may increase melt temperature by 5–10 °C relative to smooth-bore extruders. Production-scale observations indicate that melt temperature spikes above 230 °C are associated with polyethylene degradation at the head wall, black specks in the parison, and a reduction in pinch-off weld dart-drop performance.
For multi-layer coextrusion, DMDA8920 can function as a structural layer, but its viscosity must be matched to tie layers and barrier resins. A mismatch in shear viscosity at the die temperature can cause interfacial instability and wavy layer distribution. Capillary rheometry on all layers at shear rates representative of the die gap—often 100–1,000 s⁻¹ for large-part blow moulding—is required. Published data for coextruded structures containing this specific Shanxi PCEC grade is limited; laboratory-scale flat-die coextrusion trials are recommended before modifying an existing production tool.
For containers exposed to low-temperature impact below -20 °C, notched impact data under ISO 179-1/1eA may be supplemented by instrumented puncture testing at -30 °C on panels cut from the container sidewall. Performance depends on cooling rate during moulding; rapid quenching produces smaller spherulites and improves ductility but increases frozen-in stress. Where dimensional tolerances permit, a post-mould conditioning period of 24–48 h at 23 °C ± 2 °C allows shrinkage to stabilize before dimensional inspection. Containers intended for aggressive hydrocarbon mixtures should be tested under ASTM D543 immersion conditions rather than derived from general ESCR data alone.
Shanxi PCEC HDPE DMDA8920 is supported by supplier declarations that address olefin polymer requirements for food-contact use under 21 CFR 177.1520 and European plastics regulation (EU) No 10/2011, when the finished article is evaluated for migration under the intended food simulants and time-temperature conditions. The base resin is not in itself a food-contact article; conversion conditions, regrind levels, and printing layers can change specific migration limits. In containers for hazardous chemicals, certification against UN 6.1.5 requires drop testing, hydraulic pressure testing, and leak testing on the finished container, not on the resin alone.
| Regulatory or test domain | Condition or boundary | Standard or reference |
|---|---|---|
| Olefin polymer food-contact resin | Subject to end-use temperature and food-type limits; migration testing required on finished article | 21 CFR 177.1520 |
| European food-contact plastics | Requires overall migration and specific migration evaluation under (EU) No 10/2011 Annex I and II | (EU) No 10/2011 |
| Density | Nominal 0.954 g/cm³; immersion method | ISO 1183-1 |
| Melt mass-flow rate | 0.20 g/10 min at 190 °C, 2.16 kg | ISO 1133-1 |
| Tensile yield stress | Reported near 25 MPa; type 1A specimen | ISO 527-2 |
| Flexural modulus | Reported near 1,100 MPa; three-point bending | ISO 178 |
| Environmental stress-cracking resistance | Condition A, 100% Igepal CO-630 at 50 °C | ASTM D1693 |
| Hazardous goods packaging | Applied to finished container design types, not raw pellets | UN 6.1.5 |
Regrind use is generally permitted up to 20 wt% in non-food industrial containers when the regrind is generated from clean, unpigmented DMDA8920 scrap and dried if condensation is present. Higher regrind fractions may reduce dart-drop performance and environmental stress-cracking resistance because of repeated heat history. Pigmented concentrates based on incompatible carriers should be pre-evaluated in a capillary rheometer at 210 °C before production; a decrease in melt strength above 20% relative to neat resin can indicate a change in molecular weight distribution that will alter parison programming. Additives containing free amines or strong oxidizers should be avoided where long-term stabilizer performance is required, because amine-based additives can interfere with phenolic antioxidant cycles and create discoloration at weld lines.
DMDA8920 is not intended for continuous use with hot fill above 90 °C or for pressure vessels where the hoop stress exceeds the long-term hydrostatic strength of HDPE. In fuel tank applications, permeation resistance is not provided by the base HDPE alone; multilayer construction with a barrier resin such as EVOH is necessary to meet evaporative emission requirements commonly specified under CARB or EPA test procedures. Published data for this specific configuration is limited, and finished tank certification must be performed on the coextruded structure rather than on the HDPE layer alone.
Incoming resin quality control should include melt flow rate and density on each delivery, but pellet-to-pellet oxidation can also shift color and odor. A yellowness index above -0.5 or multiple black specks per 1 kg sample may indicate thermal degradation during pelleting or contamination. Silo transfer systems with high-velocity elbows can generate fines; fines content above 500 ppm by weight can lead to feed instability on grooved-feed extruders and variable shot weight. Air conveying velocities should be limited to 20–25 m/s to reduce fines formation.
Incoming material should be stored below 40 °C and protected from direct ultraviolet exposure. Bags opened for more than 24 h in humid environments may acquire surface moisture that appears as splay or porosity in the parison; if surface moisture is suspected, a dehumidified-air hopper at 70 °C for 1–2 h is usually sufficient for natural HDPE. For black or heavily pigmented lots, melt-pressure variation during extrusion should be recorded and materials with a melt flow rate shift outside ±10% of the supplier’s nominal value should be segregated for additional testing to ISO 1133-1 and ISO 1183-1 before release to blow moulding.