| HS Code | 630094 |
| Productname | Shanghai Jinfei HDPE HHM5502 |
| Manufacturer | Shanghai Jinfei Petrochemical Co., Ltd. |
| Grade | HHM5502 |
| Polymertype | High-Density Polyethylene (HDPE) |
| Appearance | White pellets |
| Density | 0.954 g/cm³ |
| Meltflowrate | 0.35 g/10 min (190°C/2.16 kg) |
| Meltingpoint | 130-135 °C |
| Vicatsofteningtemperature | 125 °C |
| Tensilestrengthatyield | 26 MPa |
| Elongationatbreak | >600% |
| Flexuralmodulus | 1000 MPa |
| Environmentalstresscrackresistance | >1000 h |
| Brittlenesstemperature | < -70 °C |
| Hardness | 60 Shore D |
| Thermaldeformationtemperature | 75 °C |
| Waterabsorption | <0.01% |
As an accredited Shanghai Jinfei HDPE HHM5502 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Shanghai Jinfei HDPE HHM5502 typically comes in 25 kg woven bags or 1,000 kg jumbo bags for bulk shipment. |
| Container Loading (20′ FCL) | 20′ FCL container loading of Shanghai Jinfei HDPE HHM5502 resin, packed in 25kg bags, palletized, shrink-wrapped, and secured for ocean freight. |
| Shipping | Shanghai Jinfei HDPE HHM5502 is shipped as a non-hazardous thermoplastic resin in 25 kg woven bags or 1000 kg jumbo bags, palletized and stretch-wrapped. Transport in clean, dry containers at ambient temperature, away from moisture and direct sunlight. Standard sea freight; no special UN classification required. |
| Storage | Store Shanghai Jinfei HDPE HHM5502 in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, sparks, and flames. Keep original bags or containers tightly sealed to prevent moisture, dust, and contamination. Avoid extreme temperatures and prolonged UV exposure. Stack securely in limited layers to prevent deformation. Observe local regulations and the manufacturer’s safety data sheet. |
| Shelf Life | Shelf life of Shanghai Jinfei HDPE HHM5502 is typically 24 months when stored cool, dry, ventilated, sealed, away from sunlight and moisture. |
For tight-head 20–60 L UN 3H1 jerricans and open-head 120–220 L UN 1H2 drums, extrusion blow molding is the largest downstream conversion route for Shanghai Jinfei HDPE HHM5502. The high-molecular-weight copolymer architecture produces a melt that tolerates long parison hang times on accumulator-head machines while maintaining die swell control adequate for calibrated neck finishes and closure torque, two properties that cannot be optimized independently. Nominal density of 0.955 g/cm³ measured under ASTM D1505-18 and melt flow rate of 0.35 g/10 min at 190 °C/2.16 kg under ASTM D1238-20 place the grade in the high-stiffness HDPE range required for top-load and stack-load resistance under UN Model Regulations Chapter 6.1. The melt flow ratio between 21.6 kg and 2.16 kg loads is used as incoming lot control because a drift of more than ±5% from the producer reference value changes die swell, parison sag, and pinch-off weld thickness on unchanged tooling.
| Qualification area | Standard / clause | Typical control parameter or note |
|---|---|---|
| Melt flow rate | ASTM D1238-20 | 0.35 g/10 min at 190 °C/2.16 kg |
| High-load melt index | ASTM D1238-20 | 35 g/10 min at 190 °C/21.6 kg |
| Density | ASTM D1505-18 | 0.955 g/cm³ nominal |
| ESCR | ASTM D1693-18 | Condition B, 100% Igepal CO-630, target F50 > 1,000 h for UN packaging |
| Drop impact | UN Model Regulations 6.1.5.3 | pass after 24 h conditioning at −18 °C |
| Stack load | UN Model Regulations 6.1.5.5 | package-size dependent, 28 days at 40 °C |
On a 90 mm grooved-barrel extruder with 30:1 L/D and an accumulator-head design, the melt temperature measured by flush-mounted thermocouples at the head is held between 190 °C and 210 °C; screw speed is limited to 40–60 rpm to avoid shear heating beyond 230 °C, above which oxidative chain scission of the high-molecular-weight fraction generates an oxidized aldehyde odor and lowers ESCR. Die gap for these containers is set at 1.5–2.5 mm with a die land length ratio of 15:1 to 25:1, because HMW-HDPE exhibits die swell values between 30% and 55% depending on output rate and head pressure. Parison programming with 30–50 points is required to direct heavier wall sections into the top chime, bottom pinch-off, and handle attachment zones; without programming, wall thickness variation around the circumference exceeds 25% and reduces drop-impact survival at −18 °C under UN 6.1.5.3.
The bottom pinch-off is the dominant failure initiation site in production. Pinch land width of 0.5–1.5 mm and flash clearance of 0.2–0.5 mm are adjusted so that mold closure cold-welds the parison without forcing melt back into the hot interior. Blow pressure of 0.6–1.0 MPa is introduced within 1.5 s of mold close; delayed inflation allows the pinch-off bead to chill and produces a weak seam detectable by peel testing. Mold temperature is controlled at 10–30 °C with turbulent chilled water, and internal cooling air at a dew point below −20 °C is applied for 30–90 s depending on nominal wall thickness of 2.5–5.0 mm. Post-mold stack strength is verified per UN 6.1.5.5 by applying a compressive load compatible with a 3 m stack height for 28 days at 40 °C.
Within the automotive under-hood segment, windshield washer reservoirs, coolant recovery bottles, and heating-ventilation ducting are blow molded from HHM5502 where the part must survive thermal cycling from −40 °C to 110 °C without stress cracking at weld lines. The load is not stack pressure but sustained hoop stress caused by internal vapor pressure and fitting insertion forces. For a 1.8–2.5 mm nominal wall, burst pressure after hot-plate welding of the filler neck is measured at 23 °C and 80 °C; at the higher temperature, the tensile yield stress of HDPE drops from the 23 °C value by a factor that must be taken from ISO 527-2 multi-temperature testing, not by extrapolating room-temperature data. Ethylene glycol/water at 50/50 volume ratio and 105 °C attacks the amorphous tie chains at weld lines that have been oriented by mold compression; therefore coolant reservoir suppliers commonly specify ASTM D1693-18 Condition A ESCR on weld-line specimens, not only on flat plaques. Methanol and ethanol in washer fluid at 20–50 wt% reduce low-temperature impact toughness, so fittings are inserted only after the part has been conditioned at −35 °C for 4 h and tested under ISO 179-1/1eU Charpy impact.
Process requirements for under-hood reservoirs are tighter than for industrial containers because the part geometry includes convoluted bellows sections and insert bosses that interrupt the parison wall. Accumulator-head machines with 20–40 point parison programming are required; die gap is programmed from 1.0 mm at the bottom near the pinch-off to 2.5 mm at the dome and boss areas. Blow air at 0.5–0.8 MPa is introduced in two stages: a pre-blow at 0.05–0.10 MPa for 0.5–1.0 s, followed by final inflation, to avoid thinning over the corrugated zones. Mold temperature is set at 20–35 °C to reduce post-mold shrinkage below 2.0% in the longest dimension. In production, failure at the pinch-off is minimized by maintaining flash clearance below 0.3 mm and keeping mold alignment within 0.1 mm at the parting line. Continuous exposure above 110 °C without a sufficient heat stabilizer package may reduce elongation at break by more than 50% within 1,000 h; published HHM5502-specific heat-aging data for this configuration is limited, so lot validation should include ISO 527-2 tensile retention after 500 h at 110 °C.
For heavy-gauge sheet production, HHM5502 is converted into 2–10 mm sheet for cut-sheet thermoforming of returnable dunnage, rack liners, and battery spacer trays. On a 110 mm single-screw extruder with 33:1 L/D, barrier flight, and a gear pump, melt temperature is controlled between 200 °C and 220 °C; head pressure is maintained at 10–15 MPa before the screen changer to compensate for melt viscosity shifts. The polished three-roll stack is set at 70–90 °C on the middle roll, and the sheet is cooled under controlled tension to keep gauge variation below ±3% across the width. Thermoforming uses twin-sided infrared quartz heaters to bring the sheet surface to 165–180 °C as measured by infrared pyrometer; sag before vacuum application must remain below 5% of sheet width. Vacuum of 0.08 MPa and plug-assist speed of 150–250 mm/s are used for draw ratios up to 2:1; deeper draws require sheet pre-stretch and higher surface temperature, which increases sag and demands higher melt strength.
Trim scrap and start-up sheet are reintroduced at up to 20 wt%; above this level, repeated heat history reduces the high-molecular-weight tail that provides melt strength and ESCR. Production-scale granulation uses single-screw size reduction rather than twin-screw pelletizing to avoid an additional thermal cycle. Each extrusion lot is qualified by ASTM D1238-20 and ASTM D1693-18; if the melt flow rate increases by more than 15% from the virgin pellet value, regrind loading is decreased. Published data for HHM5502-specific thermoformed dunnage under repeated washdown at 80 °C is limited; validation should include ISO 4892-2 UV exposure and ASTM D638-14 tensile after 500 h. For food-contact dunnage, compliance with FDA 21 CFR 177.1520(c) must be confirmed on the finished article, not assumed from resin certification alone.
When shot size exceeds 10 kg on an accumulator-head machine, the parison length commonly exceeds 1.5 m and the process bottleneck shifts from pinch-off weld strength to parison sag control and mold closure timing. A 10 s dwell under gravity reduces the upper wall thickness by 20–40% when the die gap remains static. Programmed die gap movement across 50–100 points is therefore mandatory; the lower section is extruded with a gap of 3.0–5.0 mm while the upper section closes to 1.0–1.5 mm to compensate for sag. Melt temperature is run at the lower end, 180–200 °C, to raise melt strength, but lowering below 175 °C increases die pressure and produces melt fracture on the inner parison surface. Internal pre-blow air at 0.01–0.03 MPa is injected immediately after the parison exits the die to maintain circular cross-section and prevent collapse.
Cooling for 6–10 mm walls requires internal air at 0.4–0.7 MPa and dew point below −20 °C; without dry air, condensation creates surface dimples and increases cycle time. External mold cooling at 15–25 °C is insufficient for the inner wall zone near the top opening, so secondary internal cooling nozzles are used. Post-mold dimensional stability is assessed after 48 h conditioning at 23 °C and 50% relative humidity; shrinkage in the longest side is kept below 2.5%. For outdoor water storage, UV stabilization is achieved with 2.0–2.5 wt% carbon black masterbatch or a hindered amine light stabilizer package; ISO 4892-2 cycle A weathering is used to qualify color shift and surface embrittlement. These tanks are vented, not pressure-rated; continuous internal pressure above 0.05 MPa is outside the normal service window for monolayer HMW-HDPE blow moldings unless the wall stress is validated under ISO 9080 at 60 °C.
In agricultural, oilfield, and janitorial chemical packaging, liquid contact exposes HHM5502 to wetting agents that create environmental stress cracking below the yield point. The critical variable is not chemical dissolution but crack propagation through the tie-chain network when a surface-active agent reduces the energy required for fibril separation. ASTM D1693-18 Condition B with 100% Igepal CO-630 at 50 °C is the most frequently used incoming lot control; an F50 value above 1,000 h is commonly required for UN-certified containers, while a drop below 300 h correlates with field failures at handle weld lines. On blow molded containers, stress risers are not only the pinch-off but also sharp corners at the top chime and insert threads, so cutting specimens from the container sidewall generally underestimates risk unless the weld line is included.
Monolayer HDPE containers from HHM5502 show extended contact resistance to aqueous acids, alkalis, and polar solvents at ambient temperature, but aliphatic and aromatic hydrocarbons swell the amorphous phase and can reduce top-load strength by 10–20% after 30 days immersion at 23 °C. Strong oxidizing acids above 50 °C, halogens, and hydrocarbon-soluble organic compounds are outside the resin’s operational boundary unless barrier fluorination or multi-layer construction is used. For oxygen-sensitive formulations, permeation is controlled by container weight and surface area, not by HDPE formulation alone; if the required oxygen transmission rate is below the monolayer HDPE threshold determined by ASTM D3985-17, a polyamide barrier layer is necessary.
Batch-to-batch variance in ESCR is more sensitive to molecular weight distribution than to density; therefore converters should require ASTM D1238-20 high-load melt index and ASTM D5397-20 notched constant tensile load testing for lots exposed to aggressive surfactants. If regrind is introduced, F50 may decline by 30–50% after three regrind cycles, even when melt flow rate remains within specification; this is a known limitation of HMW-HDPE blow molding and requires regrind fraction to be limited to 15–20 wt% in UN-certified containers. Converters that handle aggressive fluid concentrates should also verify weld-line ESCR on molded parts rather than relying solely on pellet or plaque data.
Competitive Shanghai Jinfei HDPE HHM5502 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Shanghai Jinfei HDPE HHM5502 is supplied as a high-density polyethylene pellet for large-part injection moulding, extrusion blow moulding, and heavy-duty sheet or container applications. The nominal density is 0.955 g/cm³ when tested under ISO 1183-1; the melt mass-flow rate determined at 190 °C with a 2.16 kg load is 0.35 g/10 min under ISO 1133-1. This melt index places the grade in the high-molecular-weight HDPE class, where melt strength and slow crack resistance are prioritised over thin-wall filling speed. The product is delivered as cylindrical pellets with a bulk density of 0.54–0.58 g/cm³ by ASTM D1895, residual moisture below 0.01 wt%, and ash below 0.02 wt% by ISO 3451-1.
The 0.35 g/10 min melt flow rate restricts injection filling of walls below 1.5 mm but enables extrusion blow moulding of containers with parison lengths exceeding 1.2 m. On a 60 mm single-screw extruder with an L/D of 25:1, the barrel profile is maintained from 170 °C at the feed throat to 190 °C at the metering section, with the die head at 180–200 °C. In injection moulding, back pressure is held at 5–10 MPa and screw rotation is limited to 40–60 min⁻¹ on a 45 mm screw; rotation above 60 min⁻¹ elevates melt temperature by 8–12 °C through viscous dissipation. The mould temperature is normally set between 20 °C and 40 °C, and a 6 mm wall section requires 35–50 s cooling time depending on cooling channel distance from the cavity surface. The lower fluidity reduces the practical processing window for closures and thin-wall containers, but it shifts the optimal shear rate in extrusion to 100–400 s⁻¹; melt fracture risk increases above 800 s⁻¹ on sheet and pipe surfaces.
Rheological capillary data at 190 °C place the zero-shear viscosity of HHM5502 in the range of 1.5 × 10⁴ to 3.0 × 10⁴ Pa·s, approximately two to four times higher than a 4 g/10 min injection-moulding HDPE. The elevated viscosity is a direct consequence of the broad molecular weight distribution and high weight-average molecular weight, which contribute to parison stability during continuous extrusion of 220 L drum preforms. Wall-thickness variation in such preforms is typically held below ±0.4 mm when the die gap is set at 1.5–2.5 mm. If the die gap is reduced below 1.5 mm, the shear stress at the die lip can exceed 0.14 MPa and produce sharkskin surface defects that persist on the inside wall of bottles and drums. In injection moulding, low-speed filling with a profiled injection velocity of 30–50 mm/s reduces jetting and weld-line weakness in thick bosses and gussets.
The substitution increases injection pressure by 15–25% at constant melt temperature. On a 650-ton hydraulic injection-moulding machine using a 55 mm screw, peak pressure during filling of a 4.5 mm wall section is observed at 105–118 MPa, compared with 78–90 MPa for a 4 g/10 min HDPE grade. Filling time at the same velocity profile increases from 2.8 s to 4.2 s, which reduces an operator’s ability to compensate for short shots through injection speed alone. The performance gain appears in slow crack growth resistance. Notched specimens tested under ASTM D1693 in 10% Igepal at 50 °C show no failure after 300 h for HHM5502, whereas the 4 g/10 min reference grade shows an F50 between 40 h and 70 h. For pallet feet subjected to repeated point loads and exposure to floor-cleaning surfactants, this shift justifies the higher injection pressure and longer hold time.
| Property | HHM5502 | 4 g/10 min HDPE injection grade | 20 g/10 min HDPE injection grade |
|---|---|---|---|
| Melt flow rate (190 °C/2.16 kg) ISO 1133-1 | 0.35 g/10 min | 4 g/10 min | 20 g/10 min |
| Density ISO 1183-1 | 0.955 g/cm³ | 0.954 g/cm³ | 0.953 g/cm³ |
| Tensile yield stress ISO 527-2 | 28 MPa | 26 MPa | 24 MPa |
| Flexural modulus ISO 178 | 1050 MPa | 980 MPa | 900 MPa |
| Charpy notched impact ISO 179-1/1eA | 15 kJ/m² | 8 kJ/m² | 5 kJ/m² |
| ESCR F50 10% Igepal ASTM D1693 | >300 h | 40–70 h | <20 h |
| Vicat softening A50 ISO 306 | 126 °C | 124 °C | 122 °C |
Comparative values are representative commercial ranges for general-purpose HDPE grades; they are not guaranteed specifications for every lot. Lot-specific certificates of analysis from Shanghai Jinfei should be reviewed for melt flow rate, density, tensile yield stress, and notched impact. Published data for HHM5502 in very high-shear thin-wall packaging is limited, and the grade is not the primary choice for moulds with flow-path-to-wall-thickness ratios above 150:1.
The density of 0.955 g/cm³ contributes to a flexural modulus of 1050 MPa under ISO 178 and a tensile yield stress of 28 MPa under ISO 527-2. Vicat softening temperature is 126 °C under ISO 306 Method A50, supporting intermittent hot-fill at 70 °C but not continuous immersion above 60 °C in aggressive hypochlorite solutions. Environmental stress cracking resistance under ASTM D1693 exceeds 300 h F50 in 10% Igepal, which is significantly longer than many medium-flow injection-moulding grades in the same density class. However, the resin is not universally chemical resistant: concentrated nitric acid above 20% at 40 °C and selected aromatic hydrocarbons can produce mass uptake of 3–6% within 7 days, and full immersion testing under ISO 175 is required for any finished article exposed to specific chemical classes.
For food-contact applications, HHM5502 is typically accompanied by supplier documentation referencing EU 10/2011 overall migration limits and FDA 21 CFR 177.1520 for olefin polymers when a food-contact grade is ordered. Finished article compliance remains dependent on the complete masterbatch and processing-aid recipe, so migration testing under EU 10/2011 and FDA 21 CFR 177.1520 is necessary for the final container or closure. Hazardous substances restrictions are assessed under REACH Annex XVII and RoHS Directive 2011/65/EU for electrical and electronic equipment enclosures; the base polyolefin itself is typically below the 0.1 wt% threshold for restricted phthalates and heavy metals, but additive packages must be confirmed separately.
Additive modification with 2–4 wt% carbon black masterbatch is common for outdoor service; notched impact may shift by 10–18% depending on the carrier resin and dispersion quality. At −30 °C, Charpy notched impact strength falls to 4–6 kJ/m², which limits unprotected cold impact service for large-diameter industrial containers. Amine-based antistatic packages require particular evaluation because processing above 220 °C can accelerate yellowing. Pre-drying is normally unnecessary for unopened pellets; if storage humidity exceeds 80%, a 80 °C desiccant drying step for 2 h prevents surface splay on injection-moulded parts. The recommended melt temperature range is 190–220 °C, and residence time at 220 °C should be kept below 10 min to limit oxidative chain scission.
Compounding HHM5502 with 20 wt% talc or calcium carbonate increases melt viscosity and requires a co-rotating twin-screw extruder with L/D 36:1 and a side feeder placed in the downstream melting zone. Screw speed is maintained at 350–450 min⁻¹; above 450 min⁻¹ the melt temperature can exceed 230 °C, at which point oxidation induction time under ISO 11357-6 falls below 15 min. Barrel settings progress from 160 °C at the feed throat to 200 °C at the die plate, with an insertion thermocouple reading below 215 °C. Vacuum degassing at −0.08 MPa in the penultimate barrel reduces volatiles that otherwise form pinholes in blow-moulded walls. When the 215 °C melt-temperature limit is exceeded for extended runs, gel formation can reach 20 gel/m² in cast sheet after 4 h of operation, requiring a shutdown and purging cycle with a low-MFR HDPE carrier.
Lot-to-lot consistency for HHM5502 is monitored through melt flow rate and density, with typical variation of ±0.05 g/10 min for MFR and ±0.001 g/cm³ for density. Silo blending is recommended for inventory stored beyond 30 days, because surface oxidation can shift Yellowness Index by 1–3 units under ASTM D6290. Regrind can be included at 10 wt% for non-critical containers; regrind above 20 wt% lowers environmental stress cracking resistance by approximately 25–35% because repeated extrusion shear initiates chain scission and reduces the high-molecular-weight tail that distinguishes HHM5502 from lower-viscosity HDPE grades.